A lithium-rich manganese-based positive electrode material and its preparation method and application
By forming a lithium salt compound-spinel phase heterostructure and a solid electrolyte-conducting carbon-conducting carbon on a single crystal-rich lithium-manganese-based material, the problems of slow Li+ diffusion and weak redox kinetics are solved. It significantly improves the first-effect and rate performance of the material.
Patent Information
- Application Number
- CN202410962720.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-18
AI Technical Summary
Single crystal lithium-rich manganese-based materials have problems such as slow Li+ diffusion and weak redox kinetics, resulting in low first efficiency and poor rate performance. Oxygen anion redox releases lattice oxygen, resulting in irreversible Li2O, resulting in the first coulomb Inefficient.
Using the synergistic effect of the first cladding layer and the second cladding layer, the first cladding layer forms a heterostructure from a lithium salt compound and a spinel-phase lithium-manganese-based material, and the second cladding layer includes a solid electrolyte and conductive carbon, Form an ion-electron conductive network to enhance lithium ion diffusion and redox kinetic properties.
Effectively inhibit the release of lattice oxygen, improve the Li+ diffusion rate, enhance the conductive properties and redox kinetic properties of the material, and improve the first-effect, capacity and rate performance of the positive electrode material.
Smart Images

Figure CN118507700B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of batteries and relates to a lithium-rich manganese-based positive electrode material and a preparation method and application thereof. Background Art
[0002] With the global focus on reducing carbon emissions, the rapid growth of the electric vehicle market will drive the demand for high-performance battery materials. Lithium-rich manganese-based materials have attracted attention for their high energy density, low cost and good safety performance. Among them, single-crystal-like lithium-rich manganese-based materials have become a hot research direction for high-capacity lithium-rich materials due to their good particle integrity, few internal interfaces and strong mechanical stability. They can inhibit the generation of cracks and the transition from layered to spinel phases during long cycles. However, single-crystal-like lithium-rich materials have Li + The problems of slow diffusion and weak redox kinetics are manifested as low initial efficiency and poor rate performance, which seriously hinder their practical application. At the same time, lithium-rich manganese-based materials also have the following problems: while providing high capacity, oxygen anion redox releases lattice oxygen and reacts with Li in the electrolyte. + The irreversible generation of Li2O will also lead to low first coulombic efficiency.
[0003] At present, there are many modification strategies used to improve the first effect of single-crystal-like lithium-rich manganese-based materials, such as ion doping and inert coating, such as MgO, SnO2, CeO2, AlF3, CoF2, MgF2 and CePO4 coating. However, the traditional ion doping and inert coating of single-crystal-like materials cannot effectively inhibit the release of surface lattice oxygen, and the first effect is not significantly improved.
[0004] Therefore, there is an urgent need to provide a solution that can effectively improve the initial efficiency and rate performance of single-crystal-like lithium-rich manganese-based materials. Summary of the invention
[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a lithium-rich manganese-based positive electrode material and its preparation method and application. Under the synergistic effect of the first coating layer and the second coating layer, the present invention can improve the initial efficiency, capacity and rate performance of the single-crystal lithium-rich manganese-based positive electrode material.
[0006] To achieve this object, the present invention adopts the following technical solutions:
[0007] In a first aspect, the present invention provides a lithium-rich manganese-based positive electrode material, the lithium-rich manganese-based positive electrode material comprising a core, and a first coating layer and a second coating layer sequentially coated on the surface of the core from the inside to the outside;
[0008] The core includes a single-crystal-like lithium-rich manganese-based positive electrode material;
[0009] The first coating layer includes a lithium salt compound and a spinel phase lithium-rich manganese-based positive electrode material, and the lithium salt compound and the spinel phase lithium-rich manganese-based positive electrode material form a heterostructure;
[0010] The second coating layer includes a solid electrolyte and conductive carbon.
[0011] The present invention provides a lithium-rich manganese-based positive electrode material, comprising a core, a first coating layer and a second coating layer; the core comprises a quasi-single-crystal lithium-rich manganese-based positive electrode material having a layered structure; in the first coating layer, a lithium salt compound and a spinel phase lithium-rich manganese-based positive electrode material form a heterostructure, the heterostructure can effectively inhibit the release of lattice oxygen, inhibit irreversible oxygen loss, and prevent positive electrode corrosion, and the spinel phase has a three-dimensional Li + The diffusion path can promote the diffusion of lithium ions and help improve the migration rate of Li+ during the charge and discharge process; the second coating layer includes a solid electrolyte and conductive carbon. The solid electrolyte has a wide electrochemical window that can match the high-voltage positive electrode material, and has high ionic conductivity that can enhance the activity of surface lithium ions; the conductive carbon has good structural stability and electronic conductivity; the solid electrolyte and conductive carbon can form an ion-electron conductive network, which can enhance the conductivity of the material, enhance the redox kinetics, and promote the cyclic reversibility of lattice oxygen;
[0012] The present invention can improve the Li + The diffusion rate helps to ease the release of oxygen, enhance the reversibility of lattice oxygen and the intrinsic kinetic properties of the material, thereby enabling the positive electrode material to have high initial efficiency, high capacity and excellent rate performance.
[0013] Preferably, the lithium salt compound includes at least one of LiBO2, Li2SiO3, Li4SiO4, Li6Si2O7, Li3PO4, LiH2PO4, Li2SO4 and LiAlO2.
[0014] Preferably, the first coating layer comprises a spinel phase lithium-rich manganese-based positive electrode material layer and a lithium salt compound layer arranged in sequence from the inside to the outside, that is, the spinel phase lithium-rich manganese-based positive electrode material layer is closer to the core.
[0015] Preferably, the solid electrolyte includes at least one of LATP (lithium aluminum titanium phosphate), LLZO (lithium lanthanum zirconium oxide) and LLTO (lithium lanthanum titanium oxide).
[0016] Preferably, the conductive carbon includes at least one of zero-dimensional conductive carbon, one-dimensional conductive carbon and two-dimensional conductive carbon.
[0017] Preferably, the zero-dimensional conductive carbon comprises acetylene black.
[0018] Preferably, the one-dimensional conductive carbon includes carbon nanofibers and / or carbon nanotubes.
[0019] Preferably, the two-dimensional conductive carbon includes graphene.
[0020] Preferably, the mass ratio of the solid electrolyte to the conductive carbon is (2-30):1, for example, it can be 2:1, 5:1, 8:1, 10:1, 12:1, 15:1, 20:1, 25:1 or 28:1, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0021] Preferably, the specific surface area of the lithium-rich manganese-based positive electrode material is 0.5-4.0 m 2 / g, for example, it can be 0.5m 2 / g, 0.8m 2 / g, 1m 2 / g, 1.5m 2 / g, 2m 2 / g, 2.5m 2 / g, 3m 2 / g, 3.5m 2 / g or 4m 2 / g, etc., but are not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0022] It should be noted that the specific surface area of the lithium-rich manganese-based positive electrode material is measured by the BET method.
[0023] In a second aspect, the present invention provides a method for preparing the lithium-rich manganese-based positive electrode material according to the first aspect, the preparation method comprising:
[0024] (1) Mixing a quasi-single-crystal lithium-rich manganese-based material and a solid acid, and sintering to obtain an intermediate product;
[0025] (2) The intermediate product, solid electrolyte and conductive carbon are mixed and sintered to obtain the lithium-rich manganese-based positive electrode material.
[0026] In the present invention, solid acid, solid electrolyte and conductive carbon are introduced to coat the single-crystal-like lithium-rich manganese-based material. The intermediate product obtained after the solid acid is sintered is a core-shell structure, the core is a single-crystal-like lithium-rich manganese-based positive electrode material, and the shell is a lithium salt compound-spinel phase lithium-rich manganese-based positive electrode material heterostructure, and the shell corresponds to the first coating layer; after the solid electrolyte and conductive carbon are sintered, a solid electrolyte-conductive carbon coating layer, i.e., the second coating layer, is formed on the surface of the intermediate product. Under the synergistic effect of solid acid, solid electrolyte and conductive carbon, a heterostructure and an ion-electron conductive network can be constructed, which can effectively improve the first effect, capacity and rate performance of the single-crystal-like lithium-rich manganese-based material.
[0027] Among them, the principle of heterostructure formation is as follows: during the sintering process of the single-crystal-like lithium-rich manganese-based material and the solid acid, the solid acid will seize the Li on the surface of the single-crystal-like lithium-rich manganese-based material and generate a lithium salt compound by itself, while the surface of the material from which the Li ions are seized is in a lithium-deficient state. During the high-temperature sintering process, a spinel phase will be formed on the surface, and the lithium salt compound and the spinel phase will form a surface mixed phase, that is, a lithium salt compound-spinel phase lithium-rich manganese-based positive electrode material heterostructure.
[0028] Preferably, the chemical formula of the single-crystal-like lithium-rich manganese-based material is Li a Mn x Co y Ni 1-x-y O2, where 1≤a≤2, 0<x≤1, 0≤y<1, x+y≤1.
[0029] The a can be, for example, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9 or 2; the x can be, for example, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9 or 1; the y can be, for example, 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8 or 0.9, but is not limited to the listed values, and other values not listed within the numerical range are equally applicable.
[0030] Preferably, the solid acid comprises at least one of B2O3, SiO2, AlPO4 and A12(SO4)3.
[0031] Preferably, based on the mass of the quasi-single-crystal lithium-rich manganese-based material, the mass content of the solid acid is denoted as a, and a=1000-8000ppm, for example, it can be 1000ppm, 2000ppm, 3000ppm, 4000ppm, 5000ppm, 6000ppm, 7000ppm or 8000ppm, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0032] Preferably, based on the mass of the quasi-single-crystal lithium-rich manganese-based material, the mass content of the solid electrolyte is recorded as b, and b=10000-50000ppm, for example, it can be 10000ppm, 12000ppm, 15000ppm, 20000ppm, 25000ppm, 28000ppm, 30000ppm, 32000ppm, 35000ppm, 40000ppm, 42000ppm, 45000ppm or 50000ppm, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0033] Preferably, based on the mass of the quasi-single-crystal lithium-rich manganese-based material, the mass content of the conductive carbon is recorded as c, and c=1000-5000ppm, for example, it can be 1000ppm, 1500ppm, 2000ppm, 2500ppm, 3000ppm, 3500ppm, 4000ppm, 4500ppm or 5000ppm, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0034] Preferably, the specific surface area of the lithium-rich manganese-based positive electrode material is denoted by Z, with the unit being m 2 / g; the Z satisfies the following condition: 3000≤(a+b+c) / Z≤45000. The value of (a+b+c) / Z can be, for example, 3100, 3200, 3300, 3500, 4000, 5000, 8000, 10000, 15000, 20000, 25000, 30000, 35000, 40000 or 42000.
[0035] In the present invention, according to the above content, the range of Z is 0.5-4.0m 2 / g.
[0036] It should be noted that when calculating (a+b+c) / Z, the unit of Z is m 2 / g, the units of a, b and c are all ppm; the calculation is performed directly according to the values of a, b, c and Z without considering unit conversion.
[0037] In the present invention, (a+b+c) / Z represents the relationship between the coating amount and the specific surface area of the positive electrode material. When the ratio is too large, on the one hand, the production cost will increase, and on the other hand, the coating layer will be too thick and an island-shaped coating layer cannot be formed. The difficulty in electrolyte infiltration will reduce the kinetic performance. When the ratio is too small, the spinel phase structure and ion-electron conductive network formed on the surface are imperfect, which will result in the improvement effect of the positive electrode material failing to achieve the optimal effect.
[0038] As a preferred technical solution of the present invention, the preparation method specifically comprises the following steps:
[0039] (I) introducing a metal salt solution, a precipitant and a complexing agent into a reaction kettle at the same time, controlling the temperature in the reaction kettle to be 40-70° C. and the pH value to be 9-12, and performing a coprecipitation reaction. After reacting for 6-24 hours, filtering, washing and drying the obtained coprecipitation product, and then sieving it through a 300-400 mesh screen to obtain a single-crystal-like lithium-rich manganese-based precursor;
[0040] The total metal ion concentration in the metal salt solution is 1-3 mol / L; the quasi-single-crystal lithium-rich manganese-based precursor includes a hydroxide precursor or a carbonate precursor; the particle size D50 of the quasi-single-crystal lithium-rich manganese-based precursor is 2.0-5.0 μm, and the tap density (TD) is 0.8-1.5 g / cm 3 , BET specific surface area is 20-50m 2 / g;
[0041] (II) Mixing the quasi-single-crystal lithium-rich manganese-based precursor and lithium salt, and sintering at 1100° C. for 12 hours in an air atmosphere to obtain a quasi-single-crystal lithium-rich manganese-based material; the chemical formula of the quasi-single-crystal lithium-rich manganese-based material is Li a Mn x Co y Ni 1-x-y O2, where 1≤a≤2, 0<x≤1, 0≤y<1, x+y≤1;
[0042] (III) mixing the quasi-single-crystal lithium-rich manganese-based material and a solid acid, sintering at 300-800°C (e.g., 350°C, 400°C, 500°C, 600°C, 700°C or 800°C, etc.) for 4-8h (e.g., 4h, 5h, 6h or 7h, etc.) to obtain an intermediate product; then mixing the intermediate product, a solid electrolyte and conductive carbon, sintering at 200-700°C (e.g., 250°C, 300°C, 350°C, 400°C, 500°C, 600°C or 700°C, etc.) for 1-7h (e.g., 1h, 2h, 3h, 5h, 6h or 7h, etc.) to obtain the lithium-rich manganese-based positive electrode material;
[0043] Wherein, the solid acid includes at least one of B2O3, SiO2, AlPO4 and A12(SO4)3; based on the mass of the quasi-single-crystal lithium-rich manganese-based material, the mass content of the solid acid is denoted as a, and a=1000-8000ppm; based on the mass of the quasi-single-crystal lithium-rich manganese-based material, the mass content of the solid electrolyte is denoted as b, and b=10000-50000ppm; based on the mass of the quasi-single-crystal lithium-rich manganese-based material, the mass content of the conductive carbon is denoted as c, and c=1000-5000ppm; the specific surface area of the lithium-rich manganese-based positive electrode material is denoted as Z, and Z satisfies the following conditions: 3000≤(a+b+c) / Z≤45000.
[0044] In the present invention, the chemical formula of the single-crystal-like lithium-rich manganese-based precursor is Mn x Co y Ni 1-x-y (OH)2 or Mn x Co y Ni 1-x-yCO3, where 0<x≤1, 0≤y<1, x+y≤1.
[0045] The two sintering steps in step (III) of the present invention can be carried out normally in an air atmosphere or a nitrogen atmosphere. Considering the cost problem, it is preferred that the two sintering steps are carried out in an air atmosphere.
[0046] In a third aspect, the present invention provides a lithium-ion battery, wherein the positive electrode of the lithium-ion battery comprises the lithium-rich manganese-based positive electrode material described in the first aspect or the lithium-rich manganese-based positive electrode material prepared by the preparation method described in the second aspect.
[0047] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0048] Compared with the prior art, the present invention has the following beneficial effects:
[0049] The present invention provides a lithium-rich manganese-based positive electrode material, comprising a core, a first coating layer and a second coating layer; the core comprises a quasi-single-crystal lithium-rich manganese-based positive electrode material having a layered structure; in the first coating layer, a lithium salt compound and a spinel phase lithium-rich manganese-based positive electrode material form a heterostructure, the heterostructure can effectively inhibit the release of lattice oxygen, inhibit irreversible oxygen loss, and prevent positive electrode corrosion, and the spinel phase has a three-dimensional Li + The diffusion path can promote the diffusion of lithium ions and help improve the migration rate of Li+ during the charge and discharge process; the second coating layer includes a solid electrolyte and conductive carbon. The solid electrolyte has a wide electrochemical window that can match the high-voltage positive electrode material, and has high ionic conductivity that can enhance the activity of surface lithium ions; the conductive carbon has good structural stability and electronic conductivity; the solid electrolyte and conductive carbon can form an ion-electron conductive network, which can enhance the conductivity of the material, enhance the redox kinetics, and promote the cyclic reversibility of lattice oxygen;
[0050] The present invention can improve the Li + The diffusion rate helps to ease the release of oxygen, enhance the reversibility of lattice oxygen and the intrinsic kinetic properties of the material, thereby enabling the positive electrode material to have high initial efficiency, high capacity and excellent rate performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1 This is the XRD diffraction pattern of the lithium-rich manganese-based positive electrode material provided in Example 3 of the present invention.
[0052] Figure 2 This is a SEM image of the lithium-rich manganese-based positive electrode material provided in Example 3 of the present invention.
[0053] Figure 3 This is a SEM image of the intermediate product obtained in step (3) of Example 3 of the present invention.
[0054] Figure 4 This is a graph showing the first charge and discharge curve of a lithium-ion battery corresponding to the lithium-rich manganese-based positive electrode material provided in Example 3 of the present invention.
[0055] Figure 5 Impedance diagram of the lithium-rich manganese-based positive electrode material provided in Example 3 of the present invention and Comparative Example 1. DETAILED DESCRIPTION
[0056] The technical solution of the present invention is further illustrated below through specific implementation methods.
[0057] Example 1
[0058] This embodiment provides a method for preparing a lithium-rich manganese-based positive electrode material, the preparation method comprising:
[0059] (1) MnSO4·H2O and NiSO4·6H2O are prepared into a metal salt solution with a total metal ion concentration of 2 mol / L, sodium hydroxide solution is prepared as a precipitant, and ammonia water is prepared as a complexing agent; the metal salt solution, the precipitant and the complexing agent are introduced into a reactor at the same time, and the temperature in the reactor is controlled to be 50°C and the pH value is 11, and a coprecipitation reaction is carried out. After reacting for 20 hours, the obtained coprecipitation product is filtered, washed and dried, and then sieved with 300 mesh to obtain a single-crystal lithium-rich manganese-based precursor Mn 0.75 Ni 0.25 (OH)2, with a particle size D50 of 3.0 μm and a tap density (TD) of 1.0 g / cm 3 , BET specific surface area is 30m 2 / g;
[0060] (2) Mixing the quasi-single-crystal lithium-rich manganese-based precursor with lithium carbonate, wherein the molar ratio of the Li element in the lithium carbonate to the transition metal element in the precursor is 1.5, and sintering at 1100° C. for 12 h in an air atmosphere to obtain a quasi-single-crystal lithium-rich manganese-based material having a chemical formula of Li 1.2 Mn 0.6 Ni 0.2 O2;
[0061] (3) Mixing the single-crystal-like lithium-rich manganese-based material and a solid acid, wherein the solid acid is B2O3, and based on the mass of the single-crystal-like lithium-rich manganese-based material, the mass content of the solid acid is a=1000ppm; sintering at 300°C for 4h in an air atmosphere to obtain an intermediate product; then mixing the intermediate product, a solid electrolyte and conductive carbon, wherein the solid electrolyte is LATP, and the conductive carbon is carbon nanofibers, and based on the mass of the single-crystal-like lithium-rich manganese-based material, the mass content of the solid electrolyte is b=10000ppm, and the mass content of the conductive carbon is c=1000ppm; sintering at 300°C for 2h in an air atmosphere to obtain the lithium-rich manganese-based positive electrode material; the BET specific surface area Z of the lithium-rich manganese-based positive electrode material is 2.0m 2 / g, calculate (a+b+c) / Z=6000.
[0062] The present embodiment also provides a lithium-rich manganese-based positive electrode material prepared by the above-mentioned preparation method, wherein the lithium-rich manganese-based positive electrode material includes an inner core, and a first coating layer and a second coating layer sequentially coated on the surface of the inner core from the inside to the outside; the inner core is a quasi-single crystal lithium-rich manganese-based positive electrode material; the first coating layer is divided into a spinel phase lithium-rich manganese-based positive electrode material layer and a lithium salt compound layer sequentially arranged from the inside to the outside, the spinel phase lithium-rich manganese-based positive electrode material in the spinel phase lithium-rich manganese-based positive electrode material layer and the lithium salt compound in the lithium salt compound layer form a heterostructure, and the lithium salt compound is LiBO2; the second coating layer is a solid electrolyte and conductive carbon, the solid electrolyte is LATP, the conductive carbon is carbon nanofiber, and the mass ratio of the solid electrolyte to the conductive carbon is 10:1.
[0063] Examples 2-5 and Comparative Examples 1-16 are based on the steps of Example 1 with parameter changes, and the specific changed parameters are shown in Table 1.
[0064] Table 1
[0065]
[0066] Performance Testing
[0067] (1) XRD test and SEM test were performed on the lithium-rich manganese-based positive electrode material provided in Example 3, and SEM test was performed on the intermediate product obtained in step (3) of Example 3.
[0068] Figure 1 The XRD diffraction pattern of the lithium-rich manganese-based positive electrode material prepared in Example 3 is shown. It can be seen from the figure that it is a typical lithium-rich manganese-based positive electrode material spectrum, and no impurity peaks are observed, indicating that the coating will not affect the structure of the lithium-rich manganese-based positive electrode material.
[0069] Figure 2The SEM image of the lithium-rich manganese-based positive electrode material prepared in Example 3 is shown. It can be seen from the figure that it has a single-crystal morphology, good roundness, and a particle size between 300-700nm.
[0070] Figure 3 The SEM image of the intermediate product obtained in step (3) of Example 3 is shown, showing the morphology of the core and the first coating layer. It can be seen from the figure that the middle area between the two dotted lines is the spinel phase lithium-manganese-rich positive electrode material layer, where the material has a spinel structure; the left side of the middle area is the lithium salt compound layer, and the right side of the middle area is the core.
[0071] (2) The lithium-rich manganese-based positive electrode material provided in Examples 1-5 and Comparative Examples 1-16 is made into a positive electrode sheet, and assembled with a negative electrode sheet, a separator and an electrolyte into a lithium-ion battery. The specific steps include: preparing a lithium-rich manganese-based positive electrode material, conductive carbon black and PVDF in a ratio of 92:4:4, mixing them with NMP, and stirring them on a magnetic stirrer until they are uniform, stirring the prepared slurry with a small spoon, and then applying it to an aluminum strip using a film applicator that has been wiped clean with alcohol and blown dry, and then baking the drawn sample on a 120°C hot plate for about 5 minutes to evaporate the NMP, transferring it to an oven, and vacuum drying it at 120°C for 12 hours, and finally cutting the dried large electrode sheet into small pieces, and placing the positive electrode sheet wrapped in aluminum foil in a 120°C drying oven for more than 2 hours. Soak the gasket, spring and shell in anhydrous ethanol for 2 hours, bake them in an oven at 70°C for 3 hours, and put them in a glove box for standby use after the ethanol evaporates. When operating in a glove box, the positive electrode shell, the positive electrode sheet, the separator, the lithium sheet and the negative electrode shell are assembled in order, wherein the electrolyte is LiPF6 electrolyte, and a lithium-ion battery is obtained after assembly.
[0072] The above lithium-ion battery was subjected to electrochemical performance test: the voltage was 2.3-4.55V, the first cycle of charge and discharge was performed at 0.1C / 0.1C, and then the second cycle of charge and discharge was performed at 0.33C / 0.33C, the charge specific capacity and discharge specific capacity of the first cycle were recorded and the first efficiency was calculated, while the discharge specific capacity of the second cycle was recorded, and the ratio of the discharge specific capacity of the second cycle to the discharge specific capacity of the first cycle was calculated. The results are shown in Table 1 above.
[0073] Figure 4 The 0.1C / 0.1C first charge and discharge curve of a lithium-ion battery prepared based on the lithium-rich manganese-based positive electrode material provided in Example 3 at 2.3-4.55V is shown. As can be seen from the figure, the 0.1C discharge specific capacity is 247.7mAh / g.
[0074] As can be seen from Table 1, Comparative Example 1 is a single-crystal lithium-rich positive electrode material that is not coated, and its corresponding capacity, first effect and rate performance are poor. Comparative Examples 2-5, 6-9, and 10-13 are coated separately with B2O3, LATP, and carbon nanofibers, respectively. Compared with Comparative Example 1, the capacity, first effect, and rate performance of the material are improved, but the improvement is not obvious. Comparative Examples 14-16 are coated with two materials among B2O3, LATP, and carbon nanofibers. Compared with Comparative Examples 2-13, the coating improvement effect is better than the single coating effect; Examples 1-5 are co-coated with B2O3, LATP, and carbon nanofibers protected by the present invention. Compared with Comparative Examples 14-16, the performance is further improved, indicating that the co-coating of solid acid, solid electrolyte, and conductive carbon plays a synergistic role, indicating that the construction of solid acid heterogeneous structure and the establishment of conductive network are compatible and achievable.
[0075] (3) The lithium-rich manganese-based positive electrode materials provided in Example 3 and Comparative Example 1 were subjected to an AC impedance test, with the test parameters being a voltage amplitude of 5 mV, an amplitude of 5 mV, and a frequency range of 0.01 Hz-1 MHz.
[0076] The spectrum obtained by the AC impedance test is composed of a semicircle and a straight line: the semicircle represents the high-frequency area, and the diameter of the semicircle represents the internal resistance of the battery, which belongs to the impedance of the electrode surface. The larger the radius, the greater the impedance; the straight line represents the low-frequency area, and the slope of the straight line represents the diffusion rate of the lithium-ion battery, which belongs to Li + The diffusion impedance caused by migration in the electrode material, the larger the slope, the greater the impedance.
[0077] Figure 5 The impedance curves of the lithium-rich manganese-based positive electrode materials provided in Example 3 and Comparative Example 1 are shown. By comparison, it can be seen that the impedance of the lithium-rich manganese-based positive electrode material provided in Example 3 is reduced, indicating that the kinetic performance of the lithium-rich positive electrode material prepared by the present invention is improved.
[0078] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.
Claims
1. A lithium-rich manganese-based positive electrode material, characterized in that: The lithium-rich manganese-based positive electrode material comprises a core, and a first coating layer and a second coating layer sequentially coated on the surface of the core from the inside to the outside; The core includes a single-crystal-like lithium-rich manganese-based positive electrode material; The first coating layer includes a lithium salt compound and a spinel phase lithium-rich manganese-based positive electrode material, and the lithium salt compound and the spinel phase lithium-rich manganese-based positive electrode material form a heterostructure; The second coating layer includes a solid electrolyte and conductive carbon; the solid electrolyte includes at least one of LATP, LLZO and LLTO; The preparation method of the lithium-rich manganese-based positive electrode material comprises: (1) Mixing a quasi-single-crystal lithium-rich manganese-based material and a solid acid, and sintering to obtain an intermediate product; (2) mixing the intermediate product, solid electrolyte and conductive carbon, and sintering to obtain the lithium-rich manganese-based positive electrode material; Wherein, the chemical formula of the single-crystal-like lithium-rich manganese-based material is Li a Mn x Co y Ni 1-x-y O2, 1≤a≤2, 0<x≤1, 0≤y<1, x+y≤1; The solid acid includes at least one of B2O3, SiO2, AlPO4 and A12(SO4)3.
2. The lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: The lithium salt compound includes at least one of LiBO2, Li2SiO3, Li4SiO4, Li6Si2O7, Li3PO4, LiH2PO4, Li2SO4 and LiAlO2; The first coating layer includes a spinel phase lithium-rich manganese-based positive electrode material layer and a lithium salt compound layer arranged in sequence from the inside to the outside.
3. The lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: The conductive carbon includes at least one of zero-dimensional conductive carbon, one-dimensional conductive carbon and two-dimensional conductive carbon; The mass ratio of the solid electrolyte to the conductive carbon is (2-30):
1.
4. The lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: The specific surface area of the lithium-rich manganese-based positive electrode material is 0.5-4.0 m 2 / g.
5. The lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: Based on the mass of the quasi-single crystal lithium-rich manganese-based material, the mass content of the solid acid is recorded as a, and a=1000-8000ppm.
6. The lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: Based on the mass of the quasi-single-crystal lithium-rich manganese-based material, the mass content of the solid electrolyte is recorded as b, where b=10000-50000ppm; Based on the mass of the quasi-single-crystal lithium-rich manganese-based material, the mass content of the conductive carbon is recorded as c, and c=1000-5000ppm.
7. The lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: The specific surface area of the lithium-rich manganese-based positive electrode material is denoted as Z, in m 2 / g; said Z satisfies the following condition: 3000≤(a+b+c) / Z≤45000.
8. The lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: The preparation method specifically comprises the following steps: (I) introducing a metal salt solution, a precipitant and a complexing agent into a reaction kettle at the same time, controlling the temperature in the reaction kettle to be 40-70° C. and the pH value to be 9-12, and performing a coprecipitation reaction. After reacting for 6-24 hours, filtering, washing and drying the obtained coprecipitation product, and then sieving it through a 300-400 mesh screen to obtain a single-crystal-like lithium-rich manganese-based precursor; The total metal ion concentration in the metal salt solution is 1-3 mol / L; the quasi-single-crystal lithium-rich manganese-based precursor includes a hydroxide precursor or a carbonate precursor; the particle size D50 of the quasi-single-crystal lithium-rich manganese-based precursor is 2.0-5.0 μm, and the tap density is 0.8-1.5 g / cm 3 , BET specific surface area is 20-50m 2 / g; (II) Mixing the quasi-single-crystal lithium-rich manganese-based precursor and lithium salt, and sintering at 1100° C. for 12 hours in an air atmosphere to obtain a quasi-single-crystal lithium-rich manganese-based material; the chemical formula of the quasi-single-crystal lithium-rich manganese-based material is Li a Mn x Co y Ni 1-x-y O2, where 1≤a≤2, 0<x≤1, 0≤y<1, x+y≤1; (III) mixing the quasi-single-crystal lithium-rich manganese-based material and a solid acid, sintering at 300-800° C. for 4-8 hours to obtain an intermediate product; then mixing the intermediate product, a solid electrolyte and conductive carbon, sintering at 200-700° C. for 1-7 hours to obtain the lithium-rich manganese-based positive electrode material; Wherein, the solid acid includes at least one of B2O3, SiO2, AlPO4 and A12(SO4)3; based on the mass of the quasi-single-crystal lithium-rich manganese-based material, the mass content of the solid acid is denoted as a, and a=1000-8000ppm; based on the mass of the quasi-single-crystal lithium-rich manganese-based material, the mass content of the solid electrolyte is denoted as b, and b=10000-50000ppm; based on the mass of the quasi-single-crystal lithium-rich manganese-based material, the mass content of the conductive carbon is denoted as c, and c=1000-5000ppm; the specific surface area of the lithium-rich manganese-based positive electrode material is denoted as Z, and Z satisfies the following conditions: 3000≤(a+b+c) / Z≤45000.
9. A lithium ion battery, characterized in that: The positive electrode of the lithium-ion battery comprises the lithium-rich manganese-based positive electrode material according to any one of claims 1 to 8.