A perovskite film, preparation method and application thereof in perovskite solar cells

By using hyperbranched polyamide-amine and modified acrylate monomers to form covalent bonds and modified layers in perovskite solar cell films, the problem of surface defects of the film is solved, the photoelectric performance and stability are improved, and suitable for pertitanium Long-term and stable use of mine solar cells.

CN118510356BActive Publication Date: 2024-12-06CHONGQING ZHONGNENG OPTICAL STORAGE TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410939480.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-12-06
Estimated Expiration
2044-07-15

AI Technical Summary

Technical Problem

The existing perovskite solar cell films have surface defects after annealing, which affects their photoelectric performance and stability, resulting in low photoelectric conversion efficiency and poor long-term stability.

Method used

Hyperbranched polyamide-amine and modified acrylate monomers are used as polymer additives to form covalent bonds and modified layers through complexation reactions and cross-linking, regulate perovskite crystal growth, reduce surface defects and improve film Hydrophobicity and self-healing ability.

Benefits of technology

Effectively passivate the surface defects of perovskite films, improve their photoelectric performance and stability, and enhance the long-term use ability of perovskite solar cell devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118510356B_ABST
    Figure CN118510356B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of solar cell technology, and discloses a perovskite film, a preparation method and its application in a perovskite solar cell. The preparation method includes: mixing alkenylbithiazole, N,N'-bis(acryl)cystamine, N,N'-methylenebisacrylamide, and N-aminoethylpiperidine to obtain a hyperbranched polyamide-amine; mixing 11-(methacrylamido)undecanoic acid, functionalized polyhexamethyleneguanidine hydrochloride, trimethylolpropane trimethacrylate, and butyl methacrylate to obtain a modified acrylate monomer; adding the hyperbranched polyamide-amine and the modified acrylate monomer to a perovskite precursor solution, and reacting by spin coating, annealing, and heating to obtain a perovskite film. The perovskite film has excellent photoelectric performance and stability, and can be used for stable use in perovskite solar cell devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solar cells, and in particular to a perovskite film, a preparation method and application thereof in a perovskite solar cell. Background Art

[0002] Perovskite material is a kind of adjustable direct bandgap semiconductor material. Compared with crystalline silicon, which is an indirect bandgap semiconductor material, it has the advantages of high light absorption coefficient and large carrier diffusion distance. Perovskite solar cells usually refer to a type of solar cell that uses ABX3 type perovskite material as the light-absorbing active layer. ABX3 perovskite material has many performance advantages such as high light absorption coefficient, direct and adjustable bandgap, long carrier diffusion, rich raw material sources and low cost. It has broad application space and potential in the field of solar cells.

[0003] As the core layer of perovskite solar cells, the perovskite layer determines the photoelectric conversion efficiency and stability of solar cells. Since the optical and electrical properties of the perovskite layer are closely related to the film preparation process and interface modification technology, the research and development of the preparation of the perovskite layer has received extensive attention. In the prior art, most perovskite films prepared by the solution method are polycrystalline films, which are enriched with crystal defects on the surface and grain boundaries. After annealing, a large number of uncoordinated lead ions or lead cluster defects will appear. These defects affect the photoelectric performance and stability of the perovskite film, which is not conducive to the long-term stable use of perovskite solar cell devices.

[0004] Prior art, such as Chinese patent application CN110085747A, discloses a perovskite film, a perovskite solar cell and a method for preparing the same. A perovskite precursor solution obtained by mixing a triacrylate compound, AX and BX2 is subjected to spin coating, annealing and heat treatment to obtain a perovskite film. During the heating process, the triacrylate compound undergoes a cross-linking reaction, and the stability of the perovskite film is improved by means of the excellent air and light-heat stability of the cross-linked polymer. Although the stability of the perovskite film is improved by means of the cross-linked polymer, the problem of surface defects in the perovskite film has not been effectively improved, which affects the photoelectric conversion efficiency of the perovskite film and its application in solar cells. Summary of the invention

[0005] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a perovskite film, a preparation method and its application in a perovskite solar cell. The perovskite film has excellent photoelectric properties and stability and can be used stably in a perovskite solar cell device.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0007] A method for preparing a perovskite film comprises the following steps:

[0008] Step 1, preparing hyperbranched polyamide-amine and modified acrylate monomer;

[0009] Wherein, the preparation of hyperbranched polyamide-amine comprises the following steps:

[0010] S11: 2,2'-diamino-4,4'-bithiazole is mixed with tetrahydrofuran, triethylamine is added, and acryloyl chloride solution is added dropwise. After the addition is complete, the mixture is reacted. After the reaction is complete, the solvent tetrahydrofuran is removed by rotary evaporation to obtain alkenylbithiazole;

[0011] S12: mixing alkenylbisthiazole, N,N'-bis(acryloyl)cystamine, N,N'-methylenebisacrylamide, N-aminoethylpiperidine, methanol and water, reacting, and after the reaction, precipitating, filtering and drying to obtain a hyperbranched polyamide-amine;

[0012] Wherein, the preparation of the modified acrylate monomer comprises the following steps:

[0013] The polyhexamethylene guanidine hydrochloride and dimethyl sulfoxide are mixed and dissolved, glycidyl methacrylate is added, and the reaction is carried out. After the reaction is completed, a reaction product is obtained, and the product is purified and dried to obtain functionalized polyhexamethylene guanidine hydrochloride; 11-(methacrylamido)undecanoic acid, functionalized polyhexamethylene guanidine hydrochloride, trimethylolpropane trimethacrylate, and butyl methacrylate are mixed to obtain a modified acrylate monomer;

[0014] Step 2: Mix lead iodide, iodomethylamine, dimethyl sulfoxide, and N,N-dimethylformamide, add hyperbranched polyamide-amine and modified acrylate monomer, stir, and obtain a perovskite precursor solution after stirring evenly; spin-coat the perovskite precursor solution on a substrate, and after spin coating, anneal to obtain a crude perovskite film; heat the crude perovskite film to react, and after the reaction is completed, cool to room temperature to obtain a perovskite film.

[0015] Preferably, when preparing the hyperbranched polyamide-amine, in S11: the mass ratio of 2,2'-diamino-4,4'-bithiazole, tetrahydrofuran, triethylamine, and acryloyl chloride solution is 10:280-300:10.2-10.5:84-86, and the acryloyl chloride solution is prepared by mixing and dissolving acryloyl chloride and tetrahydrofuran in a mass ratio of 1:7; the dropwise addition conditions are: 20-30 min at 0°C; and the reaction conditions are: reacting in a nitrogen atmosphere at a temperature of -5-0°C for 6-8 h.

[0016] Preferably, when preparing the hyperbranched polyamide-amine, in S12: the mass ratio of alkenylbithiazole, N,N'-bis(acryloyl)cystamine, N,N'-methylenebisacrylamide, N-aminoethylpiperidine, methanol and water is 30-32:26-28:28-30:25-26:320-350:110-130; the reaction conditions are: reacting at a temperature of 45-50°C for 90-100h.

[0017] Preferably, when preparing the hyperbranched polyamidoamine, the precipitating agent used in the precipitation operation comprises acetone.

[0018] Preferably, in the preparation of the modified acrylate monomer: the mass ratio of polyhexamethyleneguanidine hydrochloride, dimethyl sulfoxide, and glycidyl methacrylate is 10-13:30-40:7-8; the reaction conditions are: reaction at a temperature of 60-70°C for 60-64h; the mass ratio of 11-(methacrylamido)undecanoic acid, functionalized polyhexamethyleneguanidine hydrochloride, trimethylolpropane trimethacrylate, and butyl methacrylate is 1:2:0.3-0.5:1-1.2.

[0019] Preferably, the purification operation comprises: adding acetone 3-5 times the mass of the reaction product for precipitation, filtering, taking the filter cake, adding methanol 3-5 times the mass of the filter cake for dissolution, repeating the precipitation and filtering operations.

[0020] Preferably, in the step 2, the mass ratio of lead iodide, iodomethylamine, dimethyl sulfoxide, N,N-dimethylformamide, hyperbranched polyamide-amine, and modified acrylate monomer is 66-70:23-25:22-26:75-80:0.4-0.6:0.1-0.2; the stirring conditions are: stirring at 50-60°C for 6-8h; the annealing conditions are: annealing at 100°C for 5-10min; and the heating reaction conditions are: reacting at 130-140°C for 30-35min.

[0021] The spin coating operation includes: spinning at a speed of 1000-1200 r / min for 10-15 seconds, and then continuing to spin at a speed of 4000-4800 r / min for 25-30 seconds, and adding ethyl acetate 15 seconds before the end, wherein the amount of ethyl acetate used is 5-6 times the volume of the perovskite precursor solution used during spin coating.

[0022] Preferably, a perovskite film is prepared using the perovskite film preparation method as described above.

[0023] Preferably, an application of the perovskite film as described above in a perovskite solar cell.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] In the present invention, hyperbranched polyamide-amine and modified acrylate monomers are added to the perovskite precursor solution as polymer additives, and the surface defects of the perovskite film are efficiently passivated by utilizing the comprehensive properties of the polymer such as lower volatility and better hydrophobicity.

[0026] The thiazole ring structure has excellent heat resistance and chemical stability. At the same time, the structure has two functional groups, S atoms and N atoms, which can react with lead ions to form covalent bonds, effectively regulate the microscopic environment of perovskite crystal growth, reduce defects, and thus play a role in passivating surface defects of the perovskite film. In the present invention, 2,2'-diamino-4,4'-bithiazole and acryloyl chloride undergo nucleophilic addition reaction to graft the carbon-carbon double bond structure of bithiazole. The obtained alkenyl bithiazole and N,N'-bis(acryloyl)cystamine and N,N'-methylenebisacrylamide as carbon-carbon double bond monomers are reacted with ethylamine. The 1,1-piperidine is polymerized through the Michael addition reaction to generate a polyamide-amine with a hyperbranched structure and carbon-carbon double bond termination; the two functional groups of the S atom and the N atom in the alkenylbithiazole can form a covalent bond with the lead ion; the carbonyl group and the O atom and the N atom in the secondary amine group in the hyperbranched polyamide-amine contain lone pairs of electrons, which interact with the lead ion; through the synergistic effect of the various components, the surface defects of the perovskite film can be efficiently passivated; at the same time, due to the dynamic disulfide bond in N,N'-bis(acryloyl)cystamine, the hyperbranched polyamide-amine is endowed with the ability of self-repair, and the mechanical properties of the polymer are improved;

[0027] The invention uses polyhexamethylene guanidine hydrochloride and glycidyl methacrylate to undergo a ring-opening reaction to generate functionalized polyhexamethylene guanidine hydrochloride with a carbon-carbon double bond, and then mixes the functionalized polyhexamethylene guanidine hydrochloride with 1-(methacrylamide) undecanoic acid, trimethylolpropane trimethacrylate and butyl methacrylate to prepare a modified acrylate monomer; wherein the guanidine group in the functionalized polyhexamethylene guanidine hydrochloride and the O atom in the carboxyl group of 1-(methacrylamide) undecanoic acid both have lone pairs of electrons, which can interact with lead ions to effectively passivate defects, and the alkyl long chain in 1-(methacrylamide) undecanoic acid has a hydrophobic The invention discloses a method for preparing a perovskite film having a hydrophobic property and a hydrophobic property of the polymer. The invention discloses a method for preparing a perovskite film having a hydrophobic property and a hydrophobic property of the polymer. The method comprises the steps of: adding a hyperbranched polyamide-amine and a modified acrylate monomer as polymer additives to a perovskite precursor solution, and performing a heating reaction after annealing to cause cross-linking between the hyperbranched polyamide-amine and the modified acrylate monomer through carbon-carbon double bonds, so as to form a modified layer on the surface of the perovskite film. The method can not only regulate the growth process of the perovskite crystal and passivate the surface defects of the perovskite film, but also enhance the comprehensive performance of the perovskite film as a surface modified layer, improve the photoelectric performance and stability of the perovskite film, and facilitate the long-term stable use of the perovskite solar cell device. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 is a process flow chart for preparing a perovskite film in the present invention;

[0029] Figure 2 is a schematic diagram of the reaction for preparing alkenylbithiazole in the present invention;

[0030] Figure 3 It is a contact angle bar graph of Examples 1-5 and Comparative Examples 1-2 in the contact angle test of the present invention;

[0031] Figure 4 It is a bar graph of the photoelectric conversion efficiency of samples 1-7 in the photoelectric performance test of the present invention. DETAILED DESCRIPTION

[0032] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0033] Example 1

[0034] This embodiment discloses a method for preparing a perovskite film, comprising the following steps:

[0035] Step 1, preparing hyperbranched polyamide-amine and modified acrylate monomer;

[0036] Wherein, the preparation of hyperbranched polyamide-amine comprises the following steps:

[0037] S11: 2,2'-diamino-4,4'-bithiazole is mixed with tetrahydrofuran, triethylamine is added, and acryloyl chloride solution is added dropwise at 0°C for 20 min. After the addition is completed, the mixture is reacted at -5°C in a nitrogen atmosphere for 8 h. After the reaction is completed, the solvent tetrahydrofuran is removed by rotary evaporation at 45°C to obtain alkenylbithiazole;

[0038] The mass ratio of 2,2'-diamino-4,4'-bithiazole, tetrahydrofuran, triethylamine and acryloyl chloride solution is 10:280:10.2:84, and the acryloyl chloride solution is prepared by mixing and dissolving acryloyl chloride and tetrahydrofuran in a mass ratio of 1:7.

[0039] S12: mixing alkenylbithiazole, N,N'-bis(acryloyl)cystamine, N,N'-methylenebisacrylamide, N-aminoethylpiperidine, methanol and water in a mass ratio of 30:26:28:25:320:110, reacting at 45°C for 100 hours, and after the reaction, obtaining a reaction product, adding acetone twice the mass of the reaction product for precipitation, filtering, taking the filter cake, and drying at 40°C for 24 hours to obtain a hyperbranched polyamide-amine;

[0040] Wherein, the preparation of the modified acrylate monomer comprises the following steps:

[0041] Mix polyhexamethylene guanidine hydrochloride and dimethyl sulfoxide and dissolve them, add glycidyl methacrylate, the mass ratio of polyhexamethylene guanidine hydrochloride, dimethyl sulfoxide and glycidyl methacrylate is 10:30:7, react at 60°C for 64 hours, and after the reaction is completed, obtain a reaction product, add acetone 3 times the mass of the reaction product to precipitate, filter, take the filter cake, add methanol 3 times the mass of the filter cake to dissolve, repeat the precipitation and filtering operations, and dry at room temperature for 22 hours to obtain functionalized polyhexamethylene guanidine hydrochloride; 11-(methacrylamido) undecanoic acid, functionalized polyhexamethylene guanidine hydrochloride, trimethylolpropane trimethacrylate and butyl methacrylate are mixed in a mass ratio of 1:2:0.3:1.2 to obtain a modified acrylate monomer;

[0042] Step 2: Mix lead iodide, iodomethylamine, dimethyl sulfoxide, and N,N-dimethylformamide, add hyperbranched polyamide-amine and modified acrylate monomer, stir at 50°C for 8 hours, and after stirring evenly, obtain a perovskite precursor solution; spin-coat the perovskite precursor solution on the substrate, and after spin-coating, anneal at 100°C for 5 minutes to obtain a crude perovskite film; react the crude perovskite film at 130°C for 35 minutes, and after the reaction is completed, cool to room temperature to obtain a perovskite film;

[0043] Among them, the mass ratio of lead iodide, iodomethylamine, dimethyl sulfoxide, N,N-dimethylformamide, hyperbranched polyamide-amine, and modified acrylate monomer is 70:25:26:80:0.4:0.1; the spin coating operation includes: spin coating at a speed of 1000 r / min for 15 seconds, after spin coating, continue to spin coating at a speed of 4000 r / min for 30 seconds, and add ethyl acetate dropwise 15 seconds away from the end, and the amount of ethyl acetate used is 5 times the volume of the perovskite precursor solution used during spin coating.

[0044] Example 2

[0045] This embodiment discloses a method for preparing a perovskite film, comprising the following steps:

[0046] Step 1, preparing hyperbranched polyamide-amine and modified acrylate monomer;

[0047] Wherein, the preparation of hyperbranched polyamide-amine comprises the following steps:

[0048] S11: 2,2'-diamino-4,4'-bithiazole was mixed with tetrahydrofuran, triethylamine was added, and acryloyl chloride solution was added dropwise at 0°C for 25 min. After the addition was completed, the mixture was reacted at -5°C for 8 h in a nitrogen atmosphere. After the reaction was completed, the solvent tetrahydrofuran was removed by rotary evaporation at 50°C to obtain alkenylbithiazole;

[0049] The mass ratio of 2,2'-diamino-4,4'-bithiazole, tetrahydrofuran, triethylamine and acryloyl chloride solution is 10:285:10.2:84.5, and the acryloyl chloride solution is prepared by mixing and dissolving acryloyl chloride and tetrahydrofuran in a mass ratio of 1:7.

[0050] S12: mixing alkenylbithiazole, N,N'-bis(acryloyl)cystamine, N,N'-methylenebisacrylamide, N-aminoethylpiperidine, methanol and water in a mass ratio of 30.5:26.5:28.5:25.2:325:115, reacting at 45°C for 100 hours, and after the reaction, obtaining a reaction product, adding acetone twice the mass of the reaction product for precipitation, filtering, taking the filter cake, and drying at 40°C for 24 hours to obtain a hyperbranched polyamide-amine;

[0051] Wherein, the preparation of the modified acrylate monomer comprises the following steps:

[0052] Mix polyhexamethylene guanidine hydrochloride and dimethyl sulfoxide and dissolve them, add glycidyl methacrylate, the mass ratio of polyhexamethylene guanidine hydrochloride, dimethyl sulfoxide and glycidyl methacrylate is 11:32:7.3, react at 65°C for 62 hours, and after the reaction is completed, obtain a reaction product, add acetone 3 times the mass of the reaction product to precipitate, filter, take the filter cake, add methanol 3 times the mass of the filter cake to dissolve, repeat the precipitation and filtering operations, and dry at room temperature for 24 hours to obtain functionalized polyhexamethylene guanidine hydrochloride; 11-(methacrylamido) undecanoic acid, functionalized polyhexamethylene guanidine hydrochloride, trimethylolpropane trimethacrylate and butyl methacrylate are mixed in a mass ratio of 1:2:0.35:1.15 to obtain a modified acrylate monomer;

[0053] Step 2: Mix lead iodide, iodomethylamine, dimethyl sulfoxide, and N,N-dimethylformamide, add hyperbranched polyamide-amine and modified acrylate monomer, stir at 55°C for 7 hours, and after stirring evenly, obtain a perovskite precursor solution; spin-coat the perovskite precursor solution on the substrate, and after spin-coating, anneal at 100°C for 6 minutes to obtain a crude perovskite film; react the crude perovskite film at 135°C for 33 minutes, and after the reaction is completed, cool to room temperature to obtain a perovskite film;

[0054] Among them, the mass ratio of lead iodide, iodomethylamine, dimethyl sulfoxide, N,N-dimethylformamide, hyperbranched polyamide-amine, and modified acrylate monomer is 69:24.5:25:79:0.45:0.12; the spin coating operation includes: spin coating at a speed of 1100 r / min for 13 seconds, after spin coating, continue to spin coating at a speed of 4400 r / min for 28 seconds, and add ethyl acetate dropwise 15 seconds away from the end, and the amount of ethyl acetate used is 5 times the volume of the perovskite precursor solution used during spin coating.

[0055] Example 3

[0056] This embodiment discloses a method for preparing a perovskite film, comprising the following steps:

[0057] Step 1, preparing hyperbranched polyamide-amine and modified acrylate monomer;

[0058] Wherein, the preparation of hyperbranched polyamide-amine comprises the following steps:

[0059] S11: 2,2'-diamino-4,4'-bithiazole was mixed with tetrahydrofuran, triethylamine was added, and acryloyl chloride solution was added dropwise at 0°C for 25 min. After the addition was completed, the mixture was reacted at -2°C in a nitrogen atmosphere for 7 h. After the reaction was completed, the solvent tetrahydrofuran was removed by rotary evaporation at 50°C to obtain alkenylbithiazole;

[0060] The mass ratio of 2,2'-diamino-4,4'-bithiazole, tetrahydrofuran, triethylamine and acryloyl chloride solution is 10:290:10.3:85, and the acryloyl chloride solution is prepared by mixing and dissolving acryloyl chloride and tetrahydrofuran in a mass ratio of 1:7.

[0061] S12: mixing alkenylbisthiazole, N,N'-bis(acryloyl)cystamine, N,N'-methylenebisacrylamide, N-aminoethylpiperidine, methanol and water in a mass ratio of 31:27:29:25.5:335:120, reacting at 48°C for 95h, and after the reaction, obtaining a reaction product, adding acetone twice the mass of the reaction product for precipitation, filtering, taking the filter cake, and drying at 40°C for 24h to obtain a hyperbranched polyamide-amine;

[0062] Wherein, the preparation of the modified acrylate monomer comprises the following steps:

[0063] Mix polyhexamethylene guanidine hydrochloride and dimethyl sulfoxide and dissolve them, add glycidyl methacrylate, the mass ratio of polyhexamethylene guanidine hydrochloride, dimethyl sulfoxide and glycidyl methacrylate is 12:35:7.5, react at 65°C for 62 hours, and after the reaction is completed, obtain a reaction product, add acetone 4 times the mass of the reaction product to precipitate, filter, take the filter cake, add methanol 4 times the mass of the filter cake to dissolve, repeat the precipitation and filtering operations, and dry at room temperature for 24 hours to obtain functionalized polyhexamethylene guanidine hydrochloride; 11-(methacrylamido) undecanoic acid, functionalized polyhexamethylene guanidine hydrochloride, trimethylolpropane trimethacrylate and butyl methacrylate are mixed in a mass ratio of 1:2:0.4:1.1 to obtain a modified acrylate monomer;

[0064] Step 2: Mix lead iodide, iodomethylamine, dimethyl sulfoxide, and N,N-dimethylformamide, add hyperbranched polyamide-amine and modified acrylate monomer, stir at 55°C for 7 hours, and after stirring evenly, obtain a perovskite precursor solution; spin-coat the perovskite precursor solution on a substrate, and after spin coating, anneal at 100°C for 7 minutes to obtain a crude perovskite film; react the crude perovskite film at 135°C for 33 minutes, and after the reaction is completed, cool to room temperature to obtain a perovskite film;

[0065] Among them, the mass ratio of lead iodide, iodomethylamine, dimethyl sulfoxide, N,N-dimethylformamide, hyperbranched polyamide-amine, and modified acrylate monomer is 68:24:24:78:0.5:0.15; the spin coating operation includes: spin coating at a speed of 1100 r / min for 13 seconds, after spin coating, continue to spin coating at a speed of 4400 r / min for 28 seconds, and add ethyl acetate dropwise 15 seconds away from the end, and the amount of ethyl acetate used is 5 times the volume of the perovskite precursor solution used during spin coating.

[0066] Example 4

[0067] This embodiment discloses a method for preparing a perovskite film, comprising the following steps:

[0068] Step 1, preparing hyperbranched polyamide-amine and modified acrylate monomer;

[0069] Wherein, the preparation of hyperbranched polyamide-amine comprises the following steps:

[0070] S11: 2,2'-diamino-4,4'-bithiazole was mixed with tetrahydrofuran, triethylamine was added, and acryloyl chloride solution was added dropwise at 0°C for 25 min. After the addition was completed, the mixture was reacted in a nitrogen atmosphere at 0°C for 6 h. After the reaction was completed, the solvent tetrahydrofuran was removed by rotary evaporation at 50°C to obtain alkenylbithiazole;

[0071] The mass ratio of 2,2'-diamino-4,4'-bithiazole, tetrahydrofuran, triethylamine and acryloyl chloride solution is 10:295:10.4:85.5, and the acryloyl chloride solution is prepared by mixing and dissolving acryloyl chloride and tetrahydrofuran in a mass ratio of 1:7.

[0072] S12: mixing alkenylbithiazole, N,N'-bis(acryloyl)cystamine, N,N'-methylenebisacrylamide, N-aminoethylpiperidine, methanol and water in a mass ratio of 31.5:27.5:29.5:25.8:345:125, reacting at 48°C for 95h, and after the reaction, obtaining a reaction product, adding acetone twice the mass of the reaction product for precipitation, filtering, taking the filter cake, and drying at 40°C for 24h to obtain a hyperbranched polyamide-amine;

[0073] Wherein, the preparation of the modified acrylate monomer comprises the following steps:

[0074] Mix polyhexamethylene guanidine hydrochloride and dimethyl sulfoxide and dissolve them, add glycidyl methacrylate, the mass ratio of polyhexamethylene guanidine hydrochloride, dimethyl sulfoxide and glycidyl methacrylate is 12.5:38:7.8, react at 65°C for 62 hours, and after the reaction is completed, obtain a reaction product, add acetone 5 times the mass of the reaction product to precipitate, filter, take the filter cake, add methanol 5 times the mass of the filter cake to dissolve, repeat the precipitation and filtering operations, and dry at room temperature for 25 hours to obtain functionalized polyhexamethylene guanidine hydrochloride; 11-(methacrylamido) undecanoic acid, functionalized polyhexamethylene guanidine hydrochloride, trimethylolpropane trimethacrylate and butyl methacrylate are mixed in a mass ratio of 1:2:0.45:1.05 to obtain a modified acrylate monomer;

[0075] Step 2: Mix lead iodide, iodomethylamine, dimethyl sulfoxide, and N,N-dimethylformamide, add hyperbranched polyamide-amine and modified acrylate monomer, stir at 55°C for 7 hours, and after stirring evenly, obtain a perovskite precursor solution; spin-coat the perovskite precursor solution on a substrate, and after spin coating, anneal at 100°C for 8 minutes to obtain a crude perovskite film; react the crude perovskite film at 140°C for 30 minutes, and after the reaction is completed, cool to room temperature to obtain a perovskite film;

[0076] Among them, the mass ratio of lead iodide, iodomethylamine, dimethyl sulfoxide, N,N-dimethylformamide, hyperbranched polyamide-amine, and modified acrylate monomer is 67:23.5:23:76:0.55:0.18; the spin coating operation includes: spin coating at a speed of 1200 r / min for 12 seconds, after spin coating, continue to spin coating at a speed of 4400 r / min for 30 seconds, and add ethyl acetate dropwise 15 seconds away from the end, and the amount of ethyl acetate used is 6 times the volume of the perovskite precursor solution used during spin coating.

[0077] Example 5

[0078] This embodiment discloses a method for preparing a perovskite film, comprising the following steps:

[0079] Step 1, preparing hyperbranched polyamide-amine and modified acrylate monomer;

[0080] Wherein, the preparation of hyperbranched polyamide-amine comprises the following steps:

[0081] S11: 2,2'-diamino-4,4'-bithiazole is mixed with tetrahydrofuran, triethylamine is added, and acryloyl chloride solution is added dropwise at 0°C for 30 min. After the addition is completed, the mixture is reacted at 0°C for 6 h in a nitrogen atmosphere. After the reaction is completed, the solvent tetrahydrofuran is removed by rotary evaporation at 55°C to obtain alkenylbithiazole;

[0082] The mass ratio of 2,2'-diamino-4,4'-bithiazole, tetrahydrofuran, triethylamine and acryloyl chloride solution is 10:300:10.5:86, and the acryloyl chloride solution is prepared by mixing and dissolving acryloyl chloride and tetrahydrofuran in a mass ratio of 1:7.

[0083] S12: mixing alkenylbisthiazole, N,N'-bis(acryloyl)cystamine, N,N'-methylenebisacrylamide, N-aminoethylpiperidine, methanol and water in a mass ratio of 32:28:30:26:350:130, reacting at 50°C for 90h, and after the reaction, obtaining a reaction product, adding acetone twice the mass of the reaction product for precipitation, filtering, taking the filter cake, and drying at 40°C for 24h to obtain a hyperbranched polyamide-amine;

[0084] Wherein, the preparation of the modified acrylate monomer comprises the following steps:

[0085] Mix polyhexamethylene guanidine hydrochloride and dimethyl sulfoxide and dissolve them, add glycidyl methacrylate, the mass ratio of polyhexamethylene guanidine hydrochloride, dimethyl sulfoxide and glycidyl methacrylate is 13:40:8, react at 70°C for 60 hours, and after the reaction is completed, obtain a reaction product, add acetone 5 times the mass of the reaction product to precipitate, filter, take the filter cake, add methanol 5 times the mass of the filter cake to dissolve, repeat the precipitation and filtering operations, and dry at room temperature for 26 hours to obtain functionalized polyhexamethylene guanidine hydrochloride; 11-(methacrylamido) undecanoic acid, functionalized polyhexamethylene guanidine hydrochloride, trimethylolpropane trimethacrylate and butyl methacrylate are mixed in a mass ratio of 1:2:0.5:1 to obtain a modified acrylate monomer;

[0086] Step 2: Mix lead iodide, iodomethylamine, dimethyl sulfoxide, and N,N-dimethylformamide, add hyperbranched polyamide-amine and modified acrylate monomer, stir at 60°C for 6 hours, and after stirring evenly, obtain a perovskite precursor solution; spin-coat the perovskite precursor solution on a substrate, and after spin coating, anneal at 100°C for 10 minutes to obtain a crude perovskite film; react the crude perovskite film at 140°C for 30 minutes, and after the reaction is completed, cool to room temperature to obtain a perovskite film;

[0087] Among them, the mass ratio of lead iodide, iodomethylamine, dimethyl sulfoxide, N,N-dimethylformamide, hyperbranched polyamide-amine, and modified acrylate monomer is 66:23:22:75:0.6:0.2; the spin coating operation includes: spin coating at a speed of 1200 r / min for 10 seconds, after spin coating, continue to spin coating at a speed of 4800 r / min for 25 seconds, and add ethyl acetate dropwise 15 seconds away from the end, and the amount of ethyl acetate used is 6 times the volume of the perovskite precursor solution used during spin coating.

[0088] Comparative Example 1

[0089] This comparative example discloses a method for preparing a perovskite film, comprising the following steps:

[0090] Step 1, preparing hyperbranched polyamide-amine and modified acrylate monomer;

[0091] Wherein, the preparation of hyperbranched polyamide-amine comprises the following steps:

[0092] S11: 2,2'-diamino-4,4'-bithiazole is mixed with tetrahydrofuran, triethylamine is added, and acryloyl chloride solution is added dropwise at 0°C for 20 min. After the addition is completed, the mixture is reacted at -5°C in a nitrogen atmosphere for 8 h. After the reaction is completed, the solvent tetrahydrofuran is removed by rotary evaporation at 45°C to obtain alkenylbithiazole;

[0093] The mass ratio of 2,2'-diamino-4,4'-bithiazole, tetrahydrofuran, triethylamine and acryloyl chloride solution is 10:280:10.2:84, and the acryloyl chloride solution is prepared by mixing and dissolving acryloyl chloride and tetrahydrofuran in a mass ratio of 1:7.

[0094] S12: mixing alkenylbithiazole, N,N'-bis(acryloyl)cystamine, N,N'-methylenebisacrylamide, N-aminoethylpiperidine, methanol and water in a mass ratio of 30:26:28:25:320:110, reacting at 45°C for 100 hours, and after the reaction, obtaining a reaction product, adding acetone twice the mass of the reaction product for precipitation, filtering, taking the filter cake, and drying at 40°C for 24 hours to obtain a hyperbranched polyamide-amine;

[0095] Wherein, the preparation of the modified acrylate monomer comprises the following steps:

[0096] Mix polyhexamethylene guanidine hydrochloride and dimethyl sulfoxide and dissolve them, add glycidyl methacrylate, the mass ratio of polyhexamethylene guanidine hydrochloride, dimethyl sulfoxide and glycidyl methacrylate is 10:30:7, react at 60°C for 64 hours, and after the reaction is completed, obtain a reaction product, add acetone 3 times the mass of the reaction product to precipitate, filter, take the filter cake, add methanol 3 times the mass of the filter cake to dissolve, repeat the precipitation and filtering operations, and dry at room temperature for 22 hours to obtain functionalized polyhexamethylene guanidine hydrochloride; 11-(methacrylamido) undecanoic acid, functionalized polyhexamethylene guanidine hydrochloride, trimethylolpropane trimethacrylate and butyl methacrylate are mixed in a mass ratio of 1:2:0.3:1.2 to obtain a modified acrylate monomer;

[0097] Step 2: Mix lead iodide, iodomethylamine, dimethyl sulfoxide, and N,N-dimethylformamide, add hyperbranched polyamide-amine and modified acrylate monomer, stir at 50°C for 8 hours, and after stirring evenly, obtain a perovskite precursor solution; spin-coat the perovskite precursor solution on the substrate, and after spin-coating, anneal at 100°C for 5 minutes to obtain a crude perovskite film; react the crude perovskite film at 130°C for 35 minutes, and after the reaction is completed, cool to room temperature to obtain a perovskite film;

[0098] Among them, the mass ratio of lead iodide, iodomethylamine, dimethyl sulfoxide, N,N-dimethylformamide, hyperbranched polyamide-amine, and modified acrylate monomer is 70:25:26:80:0.4:0.1; the spin coating operation includes: spin coating at a speed of 1000 r / min for 15 seconds, after spin coating, continue to spin coating at a speed of 4000 r / min for 30 seconds, and add ethyl acetate dropwise 15 seconds away from the end, and the amount of ethyl acetate used is 5 times the volume of the perovskite precursor solution used during spin coating.

[0099] Comparative Example 2

[0100] This comparative example discloses a method for preparing a perovskite film, comprising the following steps:

[0101] Step 1, preparing hyperbranched polyamide-amine and modified acrylate monomer;

[0102] Wherein, the preparation of hyperbranched polyamide-amine comprises the following steps:

[0103] S11: 2,2'-diamino-4,4'-bithiazole is mixed with tetrahydrofuran, triethylamine is added, and acryloyl chloride solution is added dropwise at 0°C for 20 min. After the addition is completed, the mixture is reacted at -5°C in a nitrogen atmosphere for 8 h. After the reaction is completed, the solvent tetrahydrofuran is removed by rotary evaporation at 45°C to obtain alkenylbithiazole;

[0104] The mass ratio of 2,2'-diamino-4,4'-bithiazole, tetrahydrofuran, triethylamine and acryloyl chloride solution is 10:280:10.2:84, and the acryloyl chloride solution is prepared by mixing and dissolving acryloyl chloride and tetrahydrofuran in a mass ratio of 1:7.

[0105] S12: mixing alkenylbithiazole, N,N'-bis(acryloyl)cystamine, N,N'-methylenebisacrylamide, N-aminoethylpiperidine, methanol and water in a mass ratio of 30:26:28:25:320:110, reacting at 45°C for 100 hours, and after the reaction, obtaining a reaction product, adding acetone twice the mass of the reaction product for precipitation, filtering, taking the filter cake, and drying at 40°C for 24 hours to obtain a hyperbranched polyamide-amine;

[0106] Wherein, the preparation of the modified acrylate monomer comprises the following steps:

[0107] Mix polyhexamethylene guanidine hydrochloride and dimethyl sulfoxide and dissolve them, add glycidyl methacrylate, the mass ratio of polyhexamethylene guanidine hydrochloride, dimethyl sulfoxide and glycidyl methacrylate is 10:30:7, react at 60°C for 64 hours, and after the reaction is completed, obtain a reaction product, add acetone 3 times the mass of the reaction product to precipitate, filter, take the filter cake, add methanol 3 times the mass of the filter cake to dissolve, repeat the precipitation and filtering operations, and dry at room temperature for 22 hours to obtain functionalized polyhexamethylene guanidine hydrochloride; 11-(methacrylamido) undecanoic acid, functionalized polyhexamethylene guanidine hydrochloride, trimethylolpropane trimethacrylate and butyl methacrylate are mixed in a mass ratio of 1:2:0.3:1.2 to obtain a modified acrylate monomer;

[0108] Step 2: Mix lead iodide, iodomethylamine, dimethyl sulfoxide, and N,N-dimethylformamide, add hyperbranched polyamide-amine and modified acrylate monomer, stir at 50°C for 8 hours, and after stirring evenly, obtain a perovskite precursor solution; spin-coat the perovskite precursor solution on the substrate, and after spin-coating, anneal at 100°C for 5 minutes to obtain a crude perovskite film; react the crude perovskite film at 130°C for 35 minutes, and after the reaction is completed, cool to room temperature to obtain a perovskite film;

[0109] Among them, the mass ratio of lead iodide, iodomethylamine, dimethyl sulfoxide, N,N-dimethylformamide, hyperbranched polyamide-amine, and modified acrylate monomer is 70:25:26:80:0.4:0.1; the spin coating operation includes: spin coating at a speed of 1000 r / min for 15 seconds, after spin coating, continue to spin coating at a speed of 4000 r / min for 30 seconds, and add ethyl acetate dropwise 15 seconds away from the end, and the amount of ethyl acetate used is 5 times the volume of the perovskite precursor solution used during spin coating.

[0110] In the above embodiments and comparative examples: 2,2'-diamino-4,4'-bithiazole is from Shanghai Aladdin Biochemical Technology Co., Ltd., with the product number D155531 and CAS number 58139-59-6; acryloyl chloride is from Shanghai MacLean Biochemical Technology Co., Ltd., with the product number A800376 and CAS number 814-68-6; N,N'-bis(acryloyl)cystamine is from Shanghai Aladdin Biochemical Technology Co., Ltd., with the product number N304128 and CAS number 60984-57-8; N,N'-methylenebisacrylamide is from, with the CAS number 110-26-9; N-aminoethylpiperidine is from Qianyan Chemical Technology Co., Ltd., with the CAS number 140 -31-8; polyhexamethylene guanidine hydrochloride is from Shanghai Aladdin Biochemical Technology Co., Ltd., item number P304024, CAS number: 57028-96-3; 11-(Methacrylamido)undecanoic acid is from Shanghai MacLean Biochemical Technology Co., Ltd., item number M983145, CAS number: 59178-93-7; lead iodide is from Wuxi Jingke Chemical Co., Ltd., CAS number: 10101-63-0; methyl ammonium iodide is from Shanghai Aladdin Biochemical Technology Co., Ltd., item number M615701, CAS number: 14965-49-2; the substrate is ITO conductive glass, from Hefei Single Crystal Material Technology Co., Ltd., with a thickness of 0.7 mm.

[0111] Test example

[0112] Perovskite solar cells were prepared based on the perovskite films prepared in Examples 1-5 and Comparative Examples 1-2, and recorded as Samples 1-7; the contact angle test was performed on the perovskite films prepared in Examples 1-5 and Comparative Examples 1-2; and the photovoltaic performance test was performed on Samples 1-7. The perovskite solar cell is composed of a substrate, a hole transport layer, a perovskite film layer, an electron transport layer, and an electrode. The specific test results are shown in Table 1:

[0113] Table 1

[0114]

[0115] In the indicators in Table 1, the photovoltaic performance test was performed as follows: at a temperature of 25°C, an average humidity of 40%, and without encapsulation of samples 1-7, using AM1.5G, 100mW / cm 2 The photovoltaic performance of samples 1-7 was measured using a Keithley 2400 in-situ meter under simulated light illumination. The voltage setting range was -1.2 V to 1.2 V, the scanning speed was 0.2 mV / s, and the effective area of ​​samples 1-7 was 0.05 cm 2 .

[0116] It can be seen from the test results in Table 1 that the perovskite film prepared by the present invention has excellent photoelectric properties and stability, and can be stably used in perovskite solar cell devices.

[0117] In hyperbranched polyamide-amine, alkenylbithiazole has two functional groups, S and N, which can form covalent bonds with lead ions; the carbonyl group and the O and N atoms in the secondary amine group in hyperbranched polyamide-amine contain lone pairs of electrons, which interact with lead ions; through the synergistic effect of each component, the surface defects of the perovskite film can be efficiently passivated. At the same time, due to the dynamic disulfide bond in N,N'-bis(acryloyl)cystamine, the hyperbranched polyamide-amine is endowed with the ability to self-repair, and the mechanical properties of the polymer are improved.

[0118] In the modified acrylate monomer, the guanidine group in the functionalized polyhexamethylene guanidine hydrochloride and the O atom in the carboxyl group of 1-(methacrylamide) undecanoic acid both have lone pairs of electrons, which can interact with lead ions and effectively passivate defects. In addition, the long alkyl chain in 1-(methacrylamide) undecanoic acid is hydrophobic, which improves the hydrophobicity of the polymer. The hyperbranched polyamide-amine and the modified acrylate monomer can be cross-linked through carbon-carbon double bonds to form a modified layer on the surface of the perovskite film, which can not only regulate the growth process of the perovskite crystal and passivate the surface defects of the perovskite film, but also can serve as a surface modification layer to enhance the comprehensive performance of the perovskite film and improve the photoelectric performance and stability of the perovskite film.

[0119] In Comparative Example 1, no hyperbranched polyamide-amine was added, and the interaction between the hyperbranched polyamide-amine and the lead ions to passivate the surface defects of the perovskite film was lacking. The photoelectric conversion rate of the perovskite film was reduced, and the photoelectric performance of Sample 6 prepared by Comparative Example 1 was lower than that of the embodiment.

[0120] No alkenylbithiazole is added to the hyperbranched polyamide-amine of Comparative Example 2, and the two functional groups of alkenylbithiazole S atom and N atom are lacking in the passivation effect on the surface defects of the perovskite film. No modified acrylate monomer is added, and the passivation effect of functionalized polyhexamethyleneguanidine hydrochloride and 1-(methacrylamido)undecanoic acid on the surface defects of the perovskite film is lacking. At the same time, since the long alkyl chain in 1-(methacrylamido)undecanoic acid can improve the hydrophobic ability of the polymer, the contact angle and photoelectric conversion rate of the perovskite film are reduced. The photoelectric performance of Sample 7 prepared by Comparative Example 2 is lower than that of the embodiment.

[0121] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a perovskite film, characterized in that: The following steps are involved: Step 1, preparing hyperbranched polyamide-amine and modified acrylate monomer; Wherein, the preparation of hyperbranched polyamide-amine comprises the following steps: S11: 2,2'-diamino-4,4'-bithiazole is mixed with tetrahydrofuran, triethylamine is added, and acryloyl chloride solution is added dropwise. After the addition is complete, the mixture is reacted. After the reaction is complete, the solvent tetrahydrofuran is removed by rotary evaporation to obtain alkenylbithiazole; The mass ratio of 2,2'-diamino-4,4'-bithiazole, tetrahydrofuran, triethylamine and acryloyl chloride solution is 10:280-300:10.2-10.5:84-86, and the acryloyl chloride solution is prepared by mixing and dissolving acryloyl chloride and tetrahydrofuran in a mass ratio of 1:7; the dropping conditions are: 20-30 minutes at 0°C; the reaction conditions are: reacting for 6-8 hours at -5-0°C in a nitrogen atmosphere; S12: mixing alkenylbisthiazole, N,N'-bis(acryloyl)cystamine, N,N'-methylenebisacrylamide, N-aminoethylpiperidine, methanol and water, reacting, and after the reaction, precipitating, filtering and drying to obtain a hyperbranched polyamide-amine; The mass ratio of alkenylbithiazole, N,N'-bis(acryloyl)cystamine, N,N'-methylenebisacrylamide, N-aminoethylpiperidine, methanol and water is 30-32:26-28:28-30:25-26:320-350:110-130; the reaction conditions are: react at 45-50°C for 90-100h; Wherein, the preparation of the modified acrylate monomer comprises the following steps: Mixing and dissolving polyhexamethylene guanidine hydrochloride and dimethyl sulfoxide, adding glycidyl methacrylate, reacting, and obtaining a reaction product after the reaction is completed, purifying, and drying to obtain functionalized polyhexamethylene guanidine hydrochloride; The mass ratio of polyhexamethyleneguanidine hydrochloride, dimethyl sulfoxide and glycidyl methacrylate is 10-13:30-40:7-8; the reaction conditions are: reacting at a temperature of 60-70°C for 60-64h; Mixing 11-(methacrylamido)undecanoic acid, functionalized polyhexamethylene guanidine hydrochloride, trimethylolpropane trimethacrylate, and butyl methacrylate to obtain a modified acrylate monomer; Step 2: Mix lead iodide, iodomethylamine, dimethyl sulfoxide, and N,N-dimethylformamide, add hyperbranched polyamide-amine and modified acrylate monomer, stir, and obtain a perovskite precursor solution after stirring evenly; spin-coat the perovskite precursor solution on a substrate, and after spin coating, anneal to obtain a crude perovskite film; heat the crude perovskite film to react, and after the reaction is completed, cool to room temperature to obtain a perovskite film; The stirring conditions are as follows: stirring at 50-60°C for 6-8h; the annealing conditions are as follows: annealing at 100°C for 5-10min; the heating reaction conditions are as follows: reacting at 130-140°C for 30-35min; the spin coating operation includes: spin coating at 1000-1200r / min for 10-15s, and after spin coating, continuing to spin coating at 4000-4800r / min for 25-30s, and adding ethyl acetate dropwise 15s after the end, and the amount of ethyl acetate used is 5-6 times the volume of the perovskite precursor solution used during spin coating.

2. The method for preparing a perovskite thin film according to claim 1, characterized in that: In the step 1, in the preparation of the modified acrylate monomer, the mass ratio of 11-(methacrylamido)undecanoic acid, functionalized polyhexamethyleneguanidine hydrochloride, trimethylolpropane trimethacrylate, and butyl methacrylate is 1:2:0.3-0.5:1-1.

2.

3. The method for preparing a perovskite thin film according to claim 1, characterized in that: In the step 2, the mass ratio of lead iodide, iodomethylamine, dimethyl sulfoxide, N,N-dimethylformamide, hyperbranched polyamide-amine, and modified acrylate monomer is 66-70:23-25:22-26:75-80:0.4-0.6:0.1-0.

2.

4. A perovskite film, characterized in that: The film is prepared by the method for preparing a perovskite film according to any one of claims 1 to 3.

5. An application of a perovskite film on a perovskite solar cell, characterized in that: A perovskite film as claimed in claim 4 is used.