A high temperature printing and dyeing defoamer and preparation method thereof
By using modified dispersed fillers in the defoamer, combined with nano-silica and carbon nanotubes, the problem of insufficient performance of traditional defoamer in high temperature and acid-base environments is solved, and efficient foam elimination and suppression is achieved to ensure Improve the stability and quality of the textile printing and dyeing process.
Patent Information
- Application Number
- CN202410987584.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-07-23
AI Technical Summary
Traditional defoaming agents are not effective in high temperature environments and have poor stability in strong acid and alkali environments, making it difficult to adapt to the extreme conditions in the textile printing and dyeing process.
Modified dispersed fillers are used, through the combination of nano-silica and carbon nanotubes, combined with modified coupling agents and polyaminosiloxanes, to enhance the high temperature resistance and acid and alkali resistance of the defoaming agent, and improve its resistance to high temperatures and acid and alkali. Environmental stability and defoaming effect.
A high-temperature printing and dyeing defoaming agent with short defoaming time, good anti-foaming effect and good stability has been achieved. It can maintain excellent performance in high temperature and strong acid and alkali environments and avoid uneven dyeing problems.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of defoamers, and in particular relates to a high-temperature printing and dyeing defoamer and a preparation method thereof. Background Art
[0002] In the textile printing and dyeing industry, the processing involves the use of a variety of auxiliaries and dyes. Among them, surfactants such as scouring agents, fixing agents, leveling agents, dispersants, and penetrants are prone to generate a large amount of foam during the stirring, transmission, and liquid material transportation process. The presence of these foams will affect the contact between the liquid and the textile, leading to problems such as uneven dyeing, which seriously affects production efficiency and product quality. Therefore, in order to solve this problem, the textile printing and dyeing industry usually needs to use physical or chemical methods to control and eliminate the generation of foam. Compared with physical methods such as static, heating or decompression to eliminate foam, adding defoamers can quickly eliminate foam and avoid the recurrence of foam. Defoamers are special chemical substances that can reduce the surface tension of the liquid, prevent the formation of foam, and quickly eliminate existing foam. By using defoamers, good contact between the liquid and the textile can be effectively maintained to ensure the smooth progress of the dyeing process and the improvement of dyeing quality.
[0003] However, traditional defoamers have certain limitations in high temperature environments. In high-temperature printing and dyeing processes, the effect of traditional defoamers may be affected, resulting in a slow defoaming speed or poor foam suppression effect. For this reason, it is necessary to develop and apply special defoamers with high temperature stability, which can maintain stable performance in high temperature environments and ensure that foam can still be effectively controlled and eliminated under extreme conditions. For example, Chinese patent CN102049153A discloses a method for preparing a special defoamer for textiles, and its raw materials include silicone paste materials, polyether silicone oil, tributyl phosphate, aluminum stearate, Tween60, AEO-3, Span60, stearic acid, sorbic acid, alkyl mineral oil, etc. The defoamer can maintain good foam suppression ability during pulping and pulping, but it has poor compatibility in the printing and dyeing system as a polyether alkane defoamer, and has poor stability in strong acid and alkali environments, and still cannot adapt well to high temperature and strong alkali environments. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention provides a high-temperature printing and dyeing defoamer, which further improves the high temperature resistance and acid and alkali resistance of the defoamer by adopting a specific modified dispersed filler, and has the advantages of short defoaming time, good antifoaming effect, good stability, etc. The present invention also provides a preparation method of the high-temperature printing and dyeing defoamer.
[0005] A high-temperature printing and dyeing defoamer, comprising the following raw materials:
[0006] Silicone oil, modified disperse filler, propylene glycol block polyether, fatty alcohol polyoxyethylene ether AEO-7, polysorbate 80, thickener, preservative and water.
[0007] Preferably, a high-temperature printing and dyeing defoamer is made from the following raw materials in parts by weight:
[0008] 60-80 parts by weight of silicone oil, 3-10 parts by weight of modified dispersed filler, 5-12 parts by weight of propylene glycol block polyether, 2-8 parts by weight of fatty alcohol polyoxyethylene ether AEO-7, 10-15 parts by weight of polysorbate 80, 1-5 parts by weight of thickener, 0.1-0.8 parts by weight of preservative and 80-120 parts by weight of water.
[0009] Preferably, the modified dispersed filler is prepared by the following method:
[0010] Under nitrogen protection, 1-5 parts by weight of styrene ethyl trimethoxy silane, 7-12 parts by weight of tert-butyl diphenyl silane and 0.02-0.08 parts by weight of Custer catalyst are mixed, heated and stirred, and distilled under reduced pressure to obtain a modified coupling agent, 5-10 parts by weight of carbon nanotubes and 20-30 parts by weight of nano silicon dioxide are added to 800-1200 parts by weight of ethanol aqueous solution for ultrasonic treatment, and then heated and 0.5-1 parts by weight of 3-(2-aminoethylamino)propyl trimethoxy silane, 0.3-0.7 parts by weight of modified coupling agent and 0.1-0.3 parts by weight of methyl orthosilicate are added, stirred, centrifuged, and dried to obtain the modified dispersed filler.
[0011] The invention uses nano silicon dioxide as a basic raw material, firstly adds carbon nanotubes (preferably carboxylated multi-walled carbon nanotubes) and uses them in combination, and utilizes the high temperature resistance, acid and alkali corrosion resistance and other characteristics of the carbon nanotubes themselves to enhance the synergy of the nano silicon dioxide, which can not only improve the high temperature resistance and acid and alkali corrosion resistance of the defoamer, but also enhance the ability of the defoamer to eliminate foam and inhibit foam generation; then the invention further modifies the defoamer by using a modified coupling agent, polyaminosiloxane and a silicon source precursor (wherein the modified coupling agent is a modified siloxane with multiple benzene ring side groups obtained by modifying styrene ethyl trimethoxy silane by a hydrosilylation reaction with tert-butyl diphenyl silane under the action of a catalyst, which can introduce a heat-resistant large-volume chain segment into the dispersed filler, thereby greatly improving the thermal stability of the defoamer; the polyaminosiloxane helps it to better combine with the foam system, so that the defoaming and anti-foaming performances are more excellent), and finally obtains the modified dispersed filler. Compared with nano-silicon dioxide, the self-made modified dispersing filler of the present invention can well improve the dispersion and stability of the defoamer in the printing and dyeing system, realize rapid dispersion, and better discharge liquid. At the same time, it can attract the hydrophobic end of the surfactant in the foam system to reduce the surfactant concentration and promote the foam to burst. It can still maintain excellent defoaming and antifoaming performance and stability under high temperature and strong acid and alkali environment, avoiding the problem of uneven dyeing.
[0012] First, the present invention introduces carbon nanotubes (especially carboxylated multi-walled carbon nanotubes) and uses their own high temperature resistance and acid and alkali corrosion resistance as synergists. Carbon nanotubes have a highly crystalline carbon structure, good stability and chemical inertness, and can maintain stability in high temperature and acid and alkali environments. At the same time, they have a large specific surface area and rich functional groups, which are conducive to interacting with other components and improving the overall high temperature resistance and acid and alkali resistance. Nano-silicon dioxide in the filler can effectively adsorb and degrade the surfactant in the foam system, thereby accelerating the rupture and dissipation of the foam, while the carbon nanotube part can enhance the anti-foaming performance of the defoamer, and the combined effect further improves the high temperature resistance and acid and alkali resistance of the defoamer.
[0013] Secondly, the present invention optimizes the structure of the filler by introducing modified coupling agents, polyaminosiloxanes and silicon source precursors. The modified coupling agent can introduce heat-resistant bulky segments, thereby enhancing the thermal stability of the filler, while the polyaminosiloxane can be better combined with the foam system to improve the anti-foaming performance of the filler. These structurally optimized components enable the filler to remain stable in high temperature and acid-base environments and better perform the function of a defoamer.
[0014] Preferably, the modified dispersed filler is prepared by the following method:
[0015] Under nitrogen protection, 1-5 parts by weight of styrene ethyl trimethoxy silane, 7-12 parts by weight of tert-butyl diphenyl silane and 0.02-0.08 parts by weight of Custer catalyst are mixed, stirred at 90-110° C. for 10-15 hours, and distilled under reduced pressure to obtain a modified coupling agent; 5-10 parts by weight of carbon nanotubes and 20-30 parts by weight of nano silicon dioxide are added to 800-1200 parts by weight of ethanol aqueous solution, ultrasonically treated for 0.2-1 hour, then heated to 70-90° C., 0.5-1 parts by weight of 3-(2-aminoethylamino)propyl trimethoxy silane, 0.3-0.7 parts by weight of modified coupling agent and 0.1-0.3 parts by weight of methyl orthosilicate are added, stirred at 70-90° C. for 5-10 hours, centrifuged, and dried to obtain the modified dispersed filler.
[0016] Preferably, the concentration of the ethanol aqueous solution is 40-60wt%.
[0017] Preferably, the ultrasonic treatment has a power of 100-300 W and a frequency of 20-40 kHz.
[0018] Preferably, the carbon nanotubes are carboxylated multi-walled carbon nanotubes.
[0019] Preferably, the organic silicone oil is one or a mixture of two or more of hydrogen silicone oil, dimethyl silicone oil, phenylmethyl silicone oil and vinyl silicone oil.
[0020] Preferably, the thickener is one or a mixture of two or more of hydroxymethyl cellulose, hydroxyethyl cellulose, sodium carboxymethyl cellulose and carrageenan.
[0021] Preferably, the preservative is any one of isothiazolinone, potassium sorbate, sodium nitrite and sodium benzoate.
[0022] The invention also provides a method for preparing the high-temperature printing and dyeing defoaming agent.
[0023] Preferably, a method for preparing a high-temperature printing and dyeing defoamer comprises the following steps:
[0024] S1: weigh 60-80 parts by weight of silicone oil, 3-10 parts by weight of modified disperse filler, 5-12 parts by weight of propylene glycol block polyether, 2-8 parts by weight of fatty alcohol polyoxyethylene ether AEO-7, 10-15 parts by weight of polysorbate 80, 1-5 parts by weight of thickener, 0.1-0.8 parts by weight of preservative and 80-120 parts by weight of water, and set aside;
[0025] S2: Mix the silicone oil, modified disperse filler and propylene glycol block polyether, stir at 100-130°C for 1-5h, cool to 50-70°C, add fatty alcohol polyoxyethylene ether AEO-7 and polysorbate 80 and continue stirring for 0.5-2h, then add thickener, preservative and water and stir for 0.5-2h, cool to room temperature to obtain the high temperature printing and dyeing defoamer.
[0026] Beneficial effects of the present invention:
[0027] The printing and dyeing defoamer prepared by the present invention further improves the high temperature resistance and acid and alkali resistance of the defoamer by adopting a modified dispersed filler made of carbon nanotubes, nano silicon dioxide, bisaminosiloxane, a modified coupling agent and methyl orthosilicate, and has the advantages of short defoaming time, good antifoaming effect, good stability, etc. DETAILED DESCRIPTION
[0028] The following will be combined with the specific embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Example 1
[0030] A method for preparing a high-temperature printing and dyeing defoamer comprises the following steps:
[0031] S1: Weigh 75 parts by weight of dimethyl silicone oil, 6 parts by weight of modified disperse filler, 8 parts by weight of propylene glycol block polyether, 6.5 parts by weight of fatty alcohol polyoxyethylene ether AEO-7, 12 parts by weight of polysorbate 80, 3 parts by weight of thickener hydroxymethyl cellulose, 0.5 parts by weight of preservative sodium benzoate and 105 parts by weight of water for later use; wherein the viscosity of dimethyl silicone oil is 1000 mPa.s, and the average molecular weight of propylene glycol block polyether is 2000;
[0032] S2: Dimethyl silicone oil, modified dispersed filler and propylene glycol block polyether are mixed, stirred at 120°C for 2.5 hours, cooled to 60°C, fatty alcohol polyoxyethylene ether AEO-7 and polysorbate 80 are added, and stirring is continued for 1 hour, and then thickener hydroxymethyl cellulose, preservative sodium benzoate and water are added, stirred for 1.5 hours, and cooled to room temperature to obtain the high temperature printing and dyeing defoaming agent.
[0033] The modified dispersed filler is prepared by the following method:
[0034] Under nitrogen protection, 2.5 parts by weight of styreneethyltrimethoxysilane (CAS: 134000-44-5), 9.5 parts by weight of tert-butyldiphenylsilane (CAS: 33729-92-9) and 0.056 parts by weight of Custer catalyst are mixed, stirred at 106° C. for 12 hours, and distilled under reduced pressure to obtain a modified coupling agent; 7.5 parts by weight of carbon nanotubes and 25 parts by weight of nano-silicon dioxide (particle size 20-40 nm) are added to 1000 parts by weight of 50wt% ethanol aqueous solution, and ultrasonicated for 0.5 hours, with an ultrasonic power of 150W and an ultrasonic frequency of 20kHz, and then heated to 82° C. and 0.8 parts by weight of 3-(2-aminoethylamino)propyltrimethoxysilane (CAS: 1760-24-3), 0.5 parts by weight of modified coupling agent and 0.2 parts by weight of methyl orthosilicate are added, stirred at 82° C. for 8.5 hours, centrifuged, and dried to obtain the modified dispersed filler. Among them, the carbon nanotubes use carboxylated multi-walled carbon nanotubes from Shanghai Haohong Biotechnology Co., Ltd., with an inner diameter of 2-5nm, an outer diameter of 5-15nm, and a length of 10-30μm.
[0035] Example 2
[0036] A method for preparing a high-temperature printing and dyeing defoamer comprises the following steps:
[0037] S1: Weigh 75 parts by weight of dimethyl silicone oil, 6 parts by weight of modified disperse filler, 8 parts by weight of propylene glycol block polyether, 6.5 parts by weight of fatty alcohol polyoxyethylene ether AEO-7, 12 parts by weight of polysorbate 80, 3 parts by weight of thickener hydroxymethyl cellulose, 0.5 parts by weight of preservative sodium benzoate and 105 parts by weight of water for later use; wherein the viscosity of dimethyl silicone oil is 1000 mPa.s, and the average molecular weight of propylene glycol block polyether is 2000;
[0038] S2: Dimethyl silicone oil, modified dispersed filler and propylene glycol block polyether are mixed, stirred at 120°C for 2.5 hours, cooled to 60°C, fatty alcohol polyoxyethylene ether AEO-7 and polysorbate 80 are added, and stirring is continued for 1 hour, and then thickener hydroxymethyl cellulose, preservative sodium benzoate and water are added, stirred for 1.5 hours, and cooled to room temperature to obtain the high temperature printing and dyeing defoaming agent.
[0039] The modified dispersed filler is prepared by the following method:
[0040] 7.5 parts by weight of carbon nanotubes and 25 parts by weight of nano-silicon dioxide (particle size 20-40 nm) are added to 1000 parts by weight of 50wt% ethanol aqueous solution and ultrasonicated for 0.5 h, with an ultrasonic power of 150 W and an ultrasonic frequency of 20 kHz, and then heated to 82°C and 1.3 parts by weight of 3-(2-aminoethylamino)propyltrimethoxysilane (CAS: 1760-24-3) and 0.2 parts by weight of methyl orthosilicate are added, stirred at 82°C for 8.5 h, centrifuged, and dried to obtain the modified dispersed filler. Among them, the carbon nanotubes are carboxylated multi-walled carbon nanotubes from Shanghai Haohong Biomedical Technology Co., Ltd., with an inner diameter of 2-5 nm, an outer diameter of 5-15 nm, and a length of 10-30 μm.
[0041] Example 3
[0042] A method for preparing a high-temperature printing and dyeing defoamer comprises the following steps:
[0043] S1: Weigh 75 parts by weight of dimethyl silicone oil, 6 parts by weight of modified disperse filler, 8 parts by weight of propylene glycol block polyether, 6.5 parts by weight of fatty alcohol polyoxyethylene ether AEO-7, 12 parts by weight of polysorbate 80, 3 parts by weight of thickener hydroxymethyl cellulose, 0.5 parts by weight of preservative sodium benzoate and 105 parts by weight of water for later use; wherein the viscosity of dimethyl silicone oil is 1000 mPa.s, and the average molecular weight of propylene glycol block polyether is 2000;
[0044] S2: Dimethyl silicone oil, modified dispersed filler and propylene glycol block polyether are mixed, stirred at 120°C for 2.5 hours, cooled to 60°C, fatty alcohol polyoxyethylene ether AEO-7 and polysorbate 80 are added, and stirring is continued for 1 hour, and then thickener hydroxymethyl cellulose, preservative sodium benzoate and water are added, stirred for 1.5 hours, and cooled to room temperature to obtain the high temperature printing and dyeing defoaming agent.
[0045] The modified dispersed filler is prepared by the following method:
[0046] 2.5 parts by weight of styreneethyltrimethoxysilane (CAS: 134000-44-5) and 9.5 parts by weight of tert-butyldiphenylsilane (CAS: 33729-92-9) are mixed to obtain a coupling agent mixture; 7.5 parts by weight of carbon nanotubes and 25 parts by weight of nano-silicon dioxide (particle size 20-40 nm) are added to 1000 parts by weight of 50wt% ethanol aqueous solution, ultrasonicated for 0.5 h, ultrasonic power 150 W, ultrasonic frequency 20 kHz, then heated to 82° C. and 0.8 parts by weight of 3-(2-aminoethylamino)propyltrimethoxysilane (CAS: 1760-24-3), 0.5 parts by weight of the coupling agent mixture and 0.2 parts by weight of methyl orthosilicate are added, stirred at 82° C. for 8.5 h, centrifuged, and dried to obtain the modified dispersed filler. Among them, the carbon nanotubes use carboxylated multi-walled carbon nanotubes from Shanghai Haohong Biotechnology Co., Ltd., with an inner diameter of 2-5nm, an outer diameter of 5-15nm, and a length of 10-30μm.
[0047] Example 4
[0048] A method for preparing a high-temperature printing and dyeing defoamer comprises the following steps:
[0049] S1: Weigh 75 parts by weight of dimethyl silicone oil, 6 parts by weight of modified disperse filler, 8 parts by weight of propylene glycol block polyether, 6.5 parts by weight of fatty alcohol polyoxyethylene ether AEO-7, 12 parts by weight of polysorbate 80, 3 parts by weight of thickener hydroxymethyl cellulose, 0.5 parts by weight of preservative sodium benzoate and 105 parts by weight of water for later use; wherein the viscosity of dimethyl silicone oil is 1000 mPa.s, and the average molecular weight of propylene glycol block polyether is 2000;
[0050] S2: Dimethyl silicone oil, modified dispersed filler and propylene glycol block polyether are mixed, stirred at 120°C for 2.5 hours, cooled to 60°C, fatty alcohol polyoxyethylene ether AEO-7 and polysorbate 80 are added, and stirring is continued for 1 hour, and then thickener hydroxymethyl cellulose, preservative sodium benzoate and water are added, stirred for 1.5 hours, and cooled to room temperature to obtain the high temperature printing and dyeing defoaming agent.
[0051] The modified dispersed filler is prepared by the following method:
[0052] Under nitrogen protection, 2.5 parts by weight of styreneethyltrimethoxysilane (CAS: 134000-44-5), 9.5 parts by weight of tert-butyldiphenylsilane (CAS: 33729-92-9) and 0.056 parts by weight of Custer catalyst are mixed, stirred at 106° C. for 12 hours, and distilled under reduced pressure to obtain a modified coupling agent; 32.5 parts by weight of nano-silicon dioxide (particle size 20-40 nm) are added to 1000 parts by weight of 50wt% ethanol aqueous solution, and ultrasonicated for 0.5 hours, with an ultrasonic power of 150W and an ultrasonic frequency of 20kHz, and then heated to 82° C. and 0.8 parts by weight of 3-(2-aminoethylamino)propyltrimethoxysilane (CAS: 1760-24-3), 0.5 parts by weight of modified coupling agent and 0.2 parts by weight of methyl orthosilicate are added, stirred at 82° C. for 8.5 hours, centrifuged, and dried to obtain the modified dispersed filler.
[0053] Example 5
[0054] A method for preparing a high-temperature printing and dyeing defoamer comprises the following steps:
[0055] S1: Weigh 75 parts by weight of dimethyl silicone oil, 6 parts by weight of nano-silicon dioxide (particle size 20-40 nm), 8 parts by weight of propylene glycol block polyether, 6.5 parts by weight of fatty alcohol polyoxyethylene ether AEO-7, 12 parts by weight of polysorbate 80, 3 parts by weight of thickener hydroxymethyl cellulose, 0.5 parts by weight of preservative sodium benzoate and 105 parts by weight of water for later use; wherein the viscosity of dimethyl silicone oil is 1000 mPa.s, and the average molecular weight of propylene glycol block polyether is 2000;
[0056] S2: Dimethyl silicone oil, nano-silica and propylene glycol block polyether are mixed, stirred at 120°C for 2.5 hours, cooled to 60°C, fatty alcohol polyoxyethylene ether AEO-7 and polysorbate 80 are added, and stirring is continued for 1 hour. Thickener hydroxymethyl cellulose, preservative sodium benzoate and water are then added and stirred for 1.5 hours. The mixture is cooled to room temperature to obtain the high-temperature printing and dyeing defoaming agent.
[0057] Test Example 1
[0058] Acid resistance test: Add 100mL phosphoric acid aqueous solution (pH=3.5) to a 300mL beaker, then add 2mL defoamer solution (defoamer and 2wt% polyacrylic acid thickener aqueous solution diluted at 1:19) and start heating. When floccules appear on the liquid surface, record the temperature, which is the precipitation temperature of the defoamer. Continue heating and boiling for 5 minutes, then cool to room temperature and observe the liquid surface state.
[0059] Alkali resistance test: Add 100mL sodium hydroxide aqueous solution (pH=12.5) to a 300mL beaker, then add 2mL defoamer solution (defoamer and 2wt% polyacrylic acid thickener aqueous solution diluted at 1:19) and start heating. Record the temperature when floccules just appear on the liquid surface, which is the precipitation temperature of the defoamer. Continue heating and boiling for 5 minutes, then cool to room temperature and observe the liquid surface state. Among them, the more +, the more serious the precipitation.
[0060] Table 1. Temperature resistance and acid and alkali resistance of defoamers
[0061]
[0062] Test Example 2
[0063] Defoaming test: Take 50mL of foaming liquid (1.0wt% sodium dodecylbenzene sulfonate aqueous solution) with a stoppered measuring cylinder, add 0.1g of defoaming agent at a constant temperature of 60℃, cover the bottle with the stopper, shake the measuring cylinder up and down 50 times at a frequency of 2 times per second and a swing of 30-35cm, let it stand and start timing, record the time taken for the foam to disappear until the liquid surface appears, and record it as the defoaming time (s). Do 5 parallel groups and take the average value.
[0064] Centrifugal stability test: Take 0.5g of defoamer and add it to 100mL of water, stir evenly, centrifuge at 3000r / min for 5min, and observe the centrifugal stability of the sample to be tested. If there is no stratification, it proves that the centrifugal stability is good.
[0065] Table 2. Defoaming time and centrifugal stability of defoamers
[0066]
[0067] It can be seen from the above test results that the high-temperature printing and dyeing defoamer prepared in Example 1 of the present invention can still maintain excellent defoaming and antifoaming performance and stability under high temperature and strong acid and alkali environment, and can avoid problems such as uneven dyeing. This is because, compared with Examples 2-5, the modified dispersed filler used in Example 1 of the present invention uses nano-silicon dioxide as the basic raw material, firstly by adding carbon nanotubes and using them in combination, the nano-silicon dioxide is enhanced by using the high temperature resistance, acid and alkali corrosion resistance and other characteristics of the carbon nanotubes themselves, which can not only improve the high temperature resistance and acid and alkali corrosion resistance of the defoamer, but also enhance the ability of the defoamer to eliminate foam and inhibit the generation of foam. Nano-silicon dioxide in the dispersed filler can effectively adsorb and degrade the surfactant in the foam system, thereby accelerating the rupture and dissipation of the foam, while the carbon nanotube part can enhance the antifoaming performance of the defoamer, and the high temperature resistance and acid and alkali resistance of the defoamer are further improved under the joint action. Then, the present invention adopts a modified coupling agent, polyaminosiloxane and a silicon source precursor for modification, and further optimizes the structure of the filler. The modified coupling agent is a modified siloxane with multiple benzene ring side groups obtained by modifying styrene ethyl trimethoxy silane through a hydrosilylation reaction with tert-butyl diphenyl silane under the action of a catalyst. Heat-resistant large-volume chain segments can be introduced into the dispersed filler, so that the thermal stability of the defoamer is greatly improved. The polyaminosiloxane helps it to be better combined with the foam system. These structurally optimized components enable the filler to remain stable in high temperature and acid-base environments, and better play the function of the defoamer.
[0068] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.
Claims
1. A high temperature printing and dyeing defoamer, It is characterized in that Made from the following ingredients: Silicone oil, modified dispersing filler, propylene glycol block polyether, fatty alcohol polyoxyethylene ether AEO-7, polysorbate 80, thickener, preservative and water; wherein the modified dispersing filler is prepared by carbon nanotubes, nano silicon dioxide, 3-(2-aminoethylamino)propyltrimethoxysilane, modified coupling agent and methyl orthosilicate; The modified coupling agent is prepared by the following method: Under nitrogen protection, 1-5 parts by weight of styreneethyltrimethoxysilane, 7-12 parts by weight of tert-butyldiphenylsilane and 0.02-0.08 parts by weight of Custer catalyst are mixed, heated and stirred, and distilled under reduced pressure to obtain a modified coupling agent.
2. The high temperature printing and dyeing defoamer according to claim 1, It is characterized in that The invention is made of the following raw materials in parts by weight: 60-80 parts by weight of silicone oil, 3-10 parts by weight of modified dispersed filler, 5-12 parts by weight of propylene glycol block polyether, 2-8 parts by weight of fatty alcohol polyoxyethylene ether AEO-7, 10-15 parts by weight of polysorbate 80, 1-5 parts by weight of thickener, 0.1-0.8 parts by weight of preservative and 80-120 parts by weight of water.
3. The high temperature printing and dyeing defoamer according to claim 1, It is characterized in that The modified dispersed filler is prepared by the following method: 5-10 parts by weight of carbon nanotubes and 20-30 parts by weight of nano-silicon dioxide are added to 800-1200 parts by weight of ethanol aqueous solution for ultrasonic treatment, and then heated and 0.5-1 parts by weight of 3-(2-aminoethylamino)propyltrimethoxysilane, 0.3-0.7 parts by weight of a modified coupling agent and 0.1-0.3 parts by weight of methyl orthosilicate are added, stirred, centrifuged and dried to obtain the modified dispersed filler.
4. The high temperature printing and dyeing defoamer according to claim 1, It is characterized in that The organic silicone oil is one of hydrogen silicone oil, dimethyl silicone oil, phenylmethyl silicone oil and vinyl silicone oil, or a mixture of two or more thereof.
5. The high temperature printing and dyeing defoamer according to claim 1, It is characterized in that The thickener is one or a mixture of two or more of hydroxymethyl cellulose, hydroxyethyl cellulose, sodium carboxymethyl cellulose and carrageenan.
6. The high temperature printing and dyeing defoamer according to claim 1, It is characterized in that The preservative is any one of isothiazolinone, potassium sorbate, sodium nitrite and sodium benzoate.
7. A method for preparing a high temperature printing and dyeing defoamer according to any one of claims 1 to 6, It is characterized in that The following steps are involved: S1: weigh 60-80 parts by weight of silicone oil, 3-10 parts by weight of modified disperse filler, 5-12 parts by weight of propylene glycol block polyether, 2-8 parts by weight of fatty alcohol polyoxyethylene ether AEO-7, 10-15 parts by weight of polysorbate 80, 1-5 parts by weight of thickener, 0.1-0.8 parts by weight of preservative and 80-120 parts by weight of water, and set aside; S2: Mix the silicone oil, modified dispersed filler and propylene glycol block polyether, stir at 100-130° C., cool to 50-70° C., add fatty alcohol polyoxyethylene ether AEO-7 and polysorbate 80 and continue stirring, then add thickener, preservative and water and stir, cool after completion, and obtain the high-temperature printing and dyeing defoaming agent.