A metal-sulfur-based semiconductor photocatalyst and preparation method thereof

By covering the surface of the 1T phase and 2H phase of tungsten disulfide nanosheets on the surface of the whole zinc thioate nanoflower, a heterostructured photocatalyst was formed, and the total zinc thioate was solved. The problem of low photocatalytic efficiency of photocatalytic materials achieves efficient photocatalytic decomposition of aquatic hydrogen under the full spectrum, improving the utilization rate and catalytic performance of solar light.

CN118513058BActive Publication Date: 2024-11-22DONGYING AISHUO MECHANICAL EQUIP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410751133.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-11-22
Estimated Expiration
2044-06-12

AI Technical Summary

Technical Problem

The existing all-indium thioate photocatalytic materials can only absorb ultraviolet light and small-range visible light, and the electrons and holes recombinate quickly, resulting in low photocatalytic efficiency, unable to effectively utilize sunlight, and unable to meet actual needs.

Method used

Using a heterostructured photocatalyst of tungsten disulfide/full zinc thiodium thioate heterostructure photocatalyst, a tungsten disulfide nanosheet mixed with 1T phase and 2H phase is formed on the surface of the tungsten zinc thioate nanoflower. Using the high charge mobility and conductivity of the 1T phase, electron hole recombination is suppressed and the separation effect of photogenerated charge is improved.

Benefits of technology

The efficiency of photocatalytic decomposition of aquatic hydrogen is significantly improved, and the utilization rate of the whole spectrum is improved. The performance of the photocatalyst reaches 30905μmol·g-1·h-1, 3.38 times that of pure total zinc thiosulfate, and the process is simple. Low cost, suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118513058B_ABST
    Figure CN118513058B_ABST
Patent Text Reader

Abstract

The present invention proposes a metal-sulfur-based semiconductor photocatalyst and a preparation method, which belongs to the technical field of catalysts. The catalyst is a tungsten disulfide nanosheet layered on the surface of zinc indium thioate nanoflowers, and a two-dimensional / two-dimensional structure formed by tungsten disulfide nanosheets and zinc indium thioate. Compared with pure zinc indium thioate, the tungsten disulfide / zinc indium thioate heterostructure photocatalyst prepared by the present invention improves the band gap of zinc indium thioate, increases active sites, promotes the separation of photogenerated electrons and holes, inhibits the recombination of electrons and holes, improves the catalytic reduction potential, and effectively improves the utilization rate of sunlight.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalysts, and in particular to a metal sulfur-based semiconductor photocatalyst and a preparation method thereof. Background Art

[0002] As one of the most important secondary energy sources, hydrogen (H 2 ) Energy is a substitute for traditional fossil energy. It has irreplaceable advantages such as cleanliness, high energy density, and diverse sources. It has attracted great research in solving global energy and environmental problems. However, the current production of hydrogen still remains in the electrolysis of water and the decomposition of mineral fuels. These production methods have low process efficiency, high energy consumption, and great pollution to the environment. Therefore, it is of great significance to explore a green hydrogen production solution. Photocatalytic technology uses light radiation to convert light energy into chemical energy, thereby realizing the catalytic process of chemical reactions. It is an ideal green technology. Photocatalytic decomposition of water to produce hydrogen is an important direction in the field of photocatalytic research. The use of photocatalytic technology to produce hydrogen provides a new energy-saving, efficient, green and environmentally friendly solution for the hydrogen production industry.

[0003] Among the many photocatalytic materials, zinc indium sulfide (ZnIn 2 S 4 ) is a new photocatalyst. As a member of the ternary metal halide, zinc indium thioate has attracted much attention due to its excellent photoelectric activity and catalytic stability. Zinc indium thioate has suitable valence band and conduction band positions, which can meet the redox potential required for most catalytic reactions. In addition, the preparation method of zinc indium thioate is relatively simple, mature and environmentally friendly, and has been widely used in the fields of photocatalytic hydrogen production, nitrogen reduction and carbon dioxide reduction. At the same time, the ultrathin nanosheet structure provides photocatalytic sites and is conducive to the construction of composite products. Despite this, zinc indium thioate is a wide bandgap semiconductor with a bandgap width of about 2.5eV. It can only be excited by ultraviolet light with a wavelength less than 450nm and a small range of visible light, so that the electrons in the valence band of zinc indium thioate transition to the conduction band to participate in the catalytic reaction. It is well known that the energy in the visible light region of the sunlight spectrum accounts for 48%, and zinc indium thioate does not respond to most visible light. At the same time, when exposed to sunlight, the electron-hole pairs excited in zinc indium thioate can easily recombine internally in the form of light and heat, which seriously restricts the application of zinc indium thioate in the field of practical photocatalysis.

[0004] Two-dimensional transition metal sulfides are metals or semimetals and semiconductors with very small band gaps, such as molybdenum sulfide, rhenium sulfide and tungsten sulfide, which have great potential in the field of photocatalysis. When two-dimensional transition metal sulfides with abundant reserves such as tungsten sulfide are directly used as photocatalysts, they are inactive for photocatalytic water decomposition to produce hydrogen. However, in the presence of photosensitizers (such as zinc perthioindate), the 1T phase of two-dimensional transition metals such as tungsten sulfide acts as an active site for hydrogen generation due to its high charge transfer ability, while inhibiting the recombination of photosensitizer electrons and holes, improving the separation of photogenerated charges, and thus becoming an excellent co-catalyst for photocatalytic water decomposition to produce hydrogen.

[0005] Few-layer WS published by Chai Bo et al. in Applied Surface Science 2 decoratingZnIn 2 S 4 with markedly promoted charge separation and photocatalytic H 2 The study loaded tungsten sulfide nanosheets onto the surface of zinc persulfoindate to improve the photocatalytic decomposition of water to produce hydrogen. However, the inventors found that the efficiency of existing photocatalysts for decomposing water to produce hydrogen is still low, the utilization rate of sunlight is low, and the performance of photocatalytic decomposition of water to produce hydrogen is insufficient, which is far from meeting actual needs. Summary of the invention

[0006] In order to solve the technical problems of existing all-sulfide zinc indium oxide photocatalytic materials that can only absorb ultraviolet light and a small range of visible light, rapid recombination of electrons and holes, and low photocatalytic efficiency, the purpose of the present invention is to provide a tungsten disulfide / all-sulfide zinc indium oxide heterostructure photocatalyst and a preparation method, which can achieve excellent photocatalytic decomposition of water to produce hydrogen performance under the full spectrum.

[0007] The technical solution of the present invention is achieved in this way:

[0008] The invention provides a metal-sulfur-based semiconductor photocatalyst. The catalyst is a tungsten disulfide nanosheet layered on the surface of a zinc indium thioate nanoflower, and a two-dimensional / two-dimensional structure formed by the tungsten disulfide nanosheet and the zinc indium thioate.

[0009] As a further improvement of the present invention, the tungsten sulfide is composed of a mixed phase of 1T and 2H, and the 1T phase is dominant. The tungsten disulfide nanosheets with 1T phase as the main phase are different from other structures in the prior art, and their excellent conductivity plays an important role in promoting the rapid transfer of photogenerated electrons and avoiding the rapid recombination of electron holes. At present, the photocatalytic material of zinc indium sulfide can only absorb ultraviolet light and a small range of visible light, the rapid recombination of electron holes and the low photocatalytic efficiency. However, the 1T phase tungsten disulfide nanosheets have high charge migration ability, can serve as active sites for hydrogen generation, and at the same time inhibit the recombination of electron holes, improve the separation effect of photogenerated charges, and are excellent co-catalysts for improving the photocatalytic performance of zinc indium sulfide.

[0010] As a further improvement of the present invention, the 1T phase accounts for 75-76%, and the 2H phase accounts for 24-25%.

[0011] As a further improvement of the present invention, the mass ratio of tungsten disulfide:zinc indium thioate is 2-17:100.

[0012] As a further improvement of the present invention, the mass ratio of tungsten disulfide:zinc indium thioate is 12:100.

[0013] The present invention further protects a method for preparing the above-mentioned metal-sulfur-based semiconductor photocatalyst, comprising:

[0014] Adding zinc chloride and indium tetrachloride tetrahydrate powder to an ethanol / water mixture, stirring and fully dissolving to prepare a first mixture;

[0015] Adding thioacetamide powder to the first mixed solution, stirring and mixing thoroughly to prepare a second mixed solution;

[0016] The second mixed solution is transferred to a reactor for reaction, and the product is calcined to obtain a zinc persulfide indium acid photocatalyst;

[0017] Adding tungsten hexachloride and thioacetamide powder to the N,N-dimethylformamide solution, stirring and mixing thoroughly to prepare a third mixed solution;

[0018] The third mixed solution is transferred to a reactor for hydrothermal reaction, and the product is calcined to obtain a tungsten disulfide nanosheet photocatalyst;

[0019] Add zinc indium thioate and tungsten disulfide nanosheets into a mortar, add n-hexane and ethanol and grind evenly to obtain a tungsten disulfide / zinc indium thioate heterostructure photocatalyst.

[0020] Further, when preparing full thioindium acid zinc, zinc chloride, indium tetrachloride tetrahydrate and thioacetamide powder are added to an ethanol / water mixture, stirred and fully dissolved, and then transferred to a hydrothermal reactor, fully reacted, cooled to room temperature, dried, calcined and ground to prepare full thioindium acid zinc. In this process, preferably, zinc chloride and indium tetrachloride tetrahydrate powder are added to an ethanol / water mixture and mixed uniformly, and then thioacetamide powder is added to avoid the formation of zinc sulfide and / or indium sulfide.

[0021] Furthermore, the amount of zinc chloride is 0.1-0.2g, preferably 0.136g; the amount of indium tetrachloride tetrahydrate is 0.5-0.6g, preferably 0.586g; the amount of thioacetamide is 0.6-0.7g, preferably 0.601g; the amount of deionized water is 40-50mL, preferably 48mL; the amount of ethanol removal is 10-15mL, preferably 12mL; the hydrothermal reactor is a 100mL reactor; the temperature of the hydrothermal reaction is 170-190°C, preferably 180°C; the hydrothermal reaction insulation time is 12-24h, preferably 20h; when preparing the first and / or second mixed solution, the stirring time is 0.5-3h, preferably 1h.

[0022] Furthermore, the second mixed solution was transferred to a reactor, and after the reaction was completed and cooled to room temperature, it was washed with deionized water and ethanol, and the washed precipitate was dried in a vacuum.

[0023] The temperature and holding time of the hydrothermal reaction process have an important influence on the acquisition of zinc thioindate. If the holding temperature is too low, the degree of crystallization is not high. If the holding temperature is too high, zinc thioindate will decompose into nanosheets, destroying the nanostructure with the largest specific surface area. Only when the temperature is 180°C, zinc thioindate nanosheets can self-aggregate to form zinc thioindate nanoflowers. If the holding time is too short, the sample yield is too low. If the holding time is too long, it will cause excess energy loss. When the holding time is 20h, the reaction of zinc thioindate is complete.

[0024] Furthermore, when preparing 1T phase tungsten disulfide, the amount of tungsten chloride used is 0.7-0.8g, preferably 0.793g; the amount of thioacetamide used is 1.5-1.6g, preferably 1.503g; the amount of N,N-dimethylformamide used is 50-80mL, preferably 60mL; when preparing the third mixed solution, the stirring time is 0.2-0.6h, preferably 0.5h. The hydrothermal reaction kettle is a 100mL reactor; the temperature of the hydrothermal reaction is 190-220°C, preferably 200°C; the heating rate of the hydrothermal reaction is 4-6°C / min, preferably 5°C / min; the holding time of the hydrothermal reaction is 20-36h, preferably 24h; the temperature and heating rate can form deformed metastable (1T) tungsten disulfide, and based on the relationship between the shear surface potential (Zeta) of tungsten disulfide and the reaction time, the Zeta potential of the tungsten disulfide tends to be stable at 24h, and the deformed metastable (1T) tungsten disulfide is successfully obtained; after the reaction, it is cooled to room temperature.

[0025] Furthermore, the third mixed solution was transferred to a reactor, and after the reaction was completed and cooled to room temperature, it was washed with deionized water and ethanol, and the washed precipitate was dried in a vacuum.

[0026] Further, tungsten disulfide and zinc persulfoindiumate are added to the mortar. The amount of n-hexane used is 3-8 mL, preferably 5 mL; the amount of ethanol used is 1-5 mL, preferably 3 mL; the complex is washed with deionized water and ethanol, and the washed precipitate is dried in vacuum.

[0027] The present invention further protects the use of the above-mentioned metal sulfur-based semiconductor photocatalyst in the photocatalytic decomposition of water to produce hydrogen. There is no related report in the prior art on the heterostructure composed of two-dimensional 1T phase tungsten disulfide nanosheets and two-dimensional all-indium sulfide zinc nanoflowers to enhance the ultraviolet visible light photocatalytic effect of all-indium sulfide zinc nanoflowers.

[0028] The present invention has the following beneficial effects:

[0029] (1) The tungsten disulfide / zinc indium thioate heterostructure photocatalyst of the present invention self-assembles under electrostatic action to form a two-dimensional / two-dimensional structure. After being loaded on the surface of zinc indium thioate nanoflowers, the efficiency of photocatalytic decomposition of water to produce hydrogen reaches 30905 μmol·g -1 ·h -1 , which is 3.38 times that of pure all-sulfoindium zinc photocatalyst.

[0030] (2) The two-dimensional zinc indium thioate nanoflowers prepared by the present invention and the tungsten disulfide / zinc indium thioate heterostructure photocatalyst with tungsten disulfide nanosheets loaded on the surface thereof have a unique two-dimensional / two-dimensional structure and are covered with 1T phase tungsten disulfide nanosheets with good conductivity on the surface: on the one hand, the structural advantages of the two-dimensional zinc indium thioate nanoflowers that are easy to combine with tungsten disulfide nanosheets and the properties of tungsten disulfide are combined to obtain enhanced light absorption capacity; on the other hand, after forming the heterostructure, the excellent electrical conductivity of tungsten disulfide is used to facilitate carrier separation and transportation, thereby enhancing the photocatalytic performance of zinc indium thioate.

[0031] (3) The present invention prepares tungsten disulfide / zinc indium thioate heterostructure photocatalyst by solvothermal method, and the synthesis process and equipment are simple, the operation process is simple, the production cost is low, the efficiency is high, the repeatability is good, and the industrial application prospect is good. The prepared tungsten disulfide / zinc indium thioate heterostructure has enhanced light absorption capacity in the ultraviolet visible region, increases the utilization rate of sunlight, and promotes the photocatalytic effect.

[0032] (4) Compared with pure zinc indium thioate, the tungsten disulfide / zinc indium thioate heterostructure photocatalyst prepared by the present invention improves the band gap of zinc indium thioate, increases the active sites, promotes the separation of photogenerated electrons and holes, inhibits the recombination of electrons and holes, increases the catalytic reduction potential, and effectively improves the utilization rate of sunlight. At the same time, the tungsten disulfide / zinc indium thioate heterostructure photocatalyst exhibits enhanced photocatalytic water decomposition hydrogen production performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0034] Figure 1 : Scanning electron microscopy (left) and transmission electron microscopy (TEM) images of the tungsten disulfide / zinc indium thioate heterostructure photocatalyst prepared in Example 4;

[0035] Figure 2 : Nitrogen adsorption and desorption diagrams (ae) and specific surface area diagram (f) of the tungsten disulfide / zinc indium thioate heterostructure photocatalysts prepared in Examples 1, 2, 3, 4, and 5.

[0036] Figure 3: A comparison diagram (a) and a band gap value diagram (b) of the ultraviolet-visible light absorption intensity of the tungsten disulfide / zinc indium thioate heterostructure photocatalysts prepared in Examples 1, 2, 3, 4, and 5.

[0037] Figure 4 : The photocatalytic decomposition of water to produce hydrogen (a) and the rate diagram (b) of the tungsten disulfide / zinc indium thioate heterostructure photocatalyst prepared in Examples 1, 2, 3, 4, and 5 under simulated sunlight. DETAILED DESCRIPTION

[0038] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] Example 1

[0040] A fully thioindate zinc nanoflower photocatalyst without loaded tungsten disulfide nanosheets, the preparation method of which is as follows:

[0041] 0.136g of zinc chloride and 0.586g of indium tetrachloride tetrahydrate were added to 60mL of ethanol solution (ethanol: water = 1: 4) and stirred for 60 minutes to prepare the first mixed solution, followed by adding 0.601g of thioacetamide to the above solution and stirring for 60min to prepare the second mixed solution. After the above treatment, the second mixed solution was transferred to a 100mL reactor, kept in a heating box at 180°C for 20h, and naturally cooled to room temperature after the heating was completed. Finally, the product was collected, cleaned, and dried to obtain yellow zinc persulfoindate.

[0042] The all-sulfoindium zinc nanoflower photocatalyst prepared in Example 1 does not load tungsten disulfide nanosheets and has a diameter of 4-5 μm (e.g. Figure 1 ), with a hollow porous structure. Although the nanoflower structure of all-sulfoindium zinc is conducive to the construction of composite catalysts and enhances the specific surface area to improve the photocatalytic activity, the photocatalyst exhibits low ultraviolet-visible light absorption capacity and a wide band gap (such as Figure 2 ), thus showing photocatalytic water decomposition and hydrogen production performance (such as Figure 4 ), which is due to the limited UV-visible light absorption ability and rapid electron-hole recombination.

[0043] Example 2

[0044] The preparation method of the tungsten disulfide / zinc indium thioate heterostructure photocatalyst with a loading mass ratio of 2% of tungsten disulfide nanosheets is as follows:

[0045] Step 1: Add 0.136g of zinc chloride and 0.586g of indium tetrachloride tetrahydrate to 60mL of ethanol solution (ethanol: water = 1:4) and stir for 60 minutes to prepare a first mixed solution, then add 0.601g of thioacetamide to the above solution and stir for 60min to prepare a second mixed solution. After the above treatment, the second mixed solution is transferred to a 100mL reactor, kept in a heating box at 180°C for 20h, and cooled naturally to room temperature after heating. Finally, the product is collected, cleaned, and dried to obtain yellow zinc persulfoindate.

[0046] Step 2: Add 0.793g of tungsten hexachloride and 1.503g of thioacetamide powder to 60mL of N,N-dimethylformamide solution and stir for 30min to fully mix to prepare the third mixed solution. After the above treatment, transfer the third mixed solution to a 100mL reactor and keep it in a heating box at 200℃ for 24h at a heating rate of 5℃ / min. After heating, cool it naturally to room temperature. Finally, collect, wash and dry the product to obtain tungsten disulfide.

[0047] Step 3: Add 2 mg of tungsten disulfide and 100 mg of zinc persulfide indium oxide powder to a mortar. Add 5 mL of n-hexane and grind to dryness, followed by 3 mL of ethanol and grind to dryness. Finally, wash the composite with deionized water and ethanol, and dry the washed precipitate in a vacuum to prepare a tungsten disulfide / zinc persulfide indium oxide heterostructure photocatalyst.

[0048] In the tungsten disulfide / zinc thioindate heterostructure photocatalyst prepared in Example 2, the loading mass ratio of tungsten disulfide nanosheets is 2%, and a very small amount of tungsten disulfide nanosheets grows on the surface of the zinc thioindate nanoflowers. Compared with the single-structure zinc thioindate nanoflowers, the very small amount of tungsten disulfide nanosheets in the tungsten disulfide / zinc thioindate heterostructure photocatalyst changes the color of the photocatalyst from yellow to light gray. The UV-visible spectrophotometer proves that its light absorption capacity is enhanced, the visible light absorption limit is slightly expanded, the band gap value is reduced, and the utilization rate of sunlight is improved (such as Figure 2 ); At the same time, the specific surface area of ​​this sample is increased, which increases the active sites for photocatalytic hydrogen production (such as Figure 3 ); In addition, due to the excellent conductivity of 1T phase tungsten disulfide, the separation of photogenerated electrons and holes in all-sulfoindium zinc oxide is promoted, which is beneficial to the transport of carriers and enhances the photocatalytic performance of the catalyst. Compared with Example 1, the tungsten disulfide / all-sulfoindium zinc oxide heterostructure photocatalyst has improved light absorption capacity under ultraviolet visible light, increased specific surface area, and also shows enhanced photocatalytic decomposition of water to produce hydrogen performance under simulated sunlight (such as Figure 4 ).

[0049] Example 3

[0050] The preparation method of the tungsten disulfide / zinc indium thioate heterostructure photocatalyst with a loading mass ratio of tungsten disulfide nanosheets of 7% is as follows:

[0051] Step 1: Add 0.136g of zinc chloride and 0.586g of indium tetrachloride tetrahydrate to 60mL of ethanol solution (ethanol: water = 1:4) and stir for 60 minutes to prepare a first mixed solution, then add 0.601g of thioacetamide to the above solution and stir for 60min to prepare a second mixed solution. After the above treatment, the second mixed solution is transferred to a 100mL reactor, kept in a heating box at 180°C for 20h, and cooled naturally to room temperature after heating. Finally, the product is collected, cleaned, and dried to obtain yellow zinc persulfoindate.

[0052] Step 2: Add 0.793g of tungsten hexachloride and 1.503g of thioacetamide powder to 60mL of N,N-dimethylformamide solution and stir for 30min to fully mix to prepare the third mixed solution. After the above treatment, transfer the third mixed solution to a 100mL reactor and keep it in a heating box at 200℃ for 24h at a heating rate of 5℃ / min. After heating, cool it naturally to room temperature. Finally, collect, wash and dry the product to obtain tungsten disulfide.

[0053] Step 3: Add 7 mg of tungsten disulfide and 100 mg of zinc persulfide indium oxide powder to a mortar. Add 5 mL of n-hexane and grind until dry, then add 3 mL of ethanol and grind until dry. Finally, wash the composite with deionized water and ethanol, and dry the washed precipitate in a vacuum to prepare a tungsten disulfide / zinc persulfide indium oxide heterostructure photocatalyst.

[0054] The tungsten disulfide / zinc indium thioate heterostructure photocatalyst prepared in the above-mentioned Example 3 has a loading mass ratio of tungsten disulfide nanosheets of 7%, and a relatively small amount of tungsten disulfide nanosheets grows on the surface of the zinc indium thioate nanoflowers. Compared with the zinc indium thioate with a single structure, the relatively small amount of tungsten disulfide nanosheets in the tungsten disulfide / zinc indium thioate heterostructure photocatalyst changes the color of the photocatalyst from yellow to a slightly darker light gray than that in Example 2. The UV-visible spectrophotometer proves that the light absorption capacity is enhanced, the visible light absorption limit is expanded, the band gap value is reduced, and the utilization rate of sunlight is improved (such as Figure 2 ); At the same time, the specific surface area of ​​this sample is increased, which increases the active sites for photocatalytic hydrogen production (such as Figure 3); In addition, due to the excellent conductivity of 1T phase tungsten disulfide, the separation of photogenerated electrons and holes in all-sulfoindium zinc oxide is promoted, which is beneficial to the transport of carriers and enhances the photocatalytic performance of the catalyst. Compared with Examples 1 and 2, the tungsten disulfide / all-sulfoindium zinc oxide heterostructure photocatalyst has improved light absorption capacity under ultraviolet visible light, increased specific surface area, and enhanced photocatalytic water decomposition hydrogen production performance under simulated sunlight (such as Figure 4 ).

[0055] Example 4

[0056] The preparation method of the tungsten disulfide / zinc indium thioate heterostructure photocatalyst with a loading mass ratio of 12% of tungsten disulfide nanosheets is as follows:

[0057] Step 1: Add 0.136g of zinc chloride and 0.586g of indium tetrachloride tetrahydrate to 60mL of ethanol solution (ethanol: water = 1:4) and stir for 60 minutes to prepare a first mixed solution, then add 0.601g of thioacetamide to the above solution and stir for 60min to prepare a second mixed solution. After the above treatment, the second mixed solution is transferred to a 100mL reactor, kept in a heating box at 180°C for 20h, and cooled naturally to room temperature after heating. Finally, the product is collected, cleaned, and dried to obtain yellow zinc persulfoindate.

[0058] Step 2: Add 0.793g of tungsten hexachloride and 1.503g of thioacetamide powder to 60mL of N,N-dimethylformamide solution and stir for 30min to fully mix to prepare the third mixed solution. After the above treatment, transfer the third mixed solution to a 100mL reactor and keep it in a heating box at 200℃ for 24h at a heating rate of 5℃ / min. After heating, cool it naturally to room temperature. Finally, collect, wash and dry the product to obtain tungsten disulfide.

[0059] Step 3: Add 12 mg of tungsten disulfide and 100 mg of zinc persulfide indium oxide powder to a mortar. Add 5 mL of n-hexane and grind until dry, then add 3 mL of ethanol and grind until dry. Finally, wash the composite with deionized water and ethanol, and dry the washed precipitate in a vacuum to prepare a tungsten disulfide / zinc persulfide indium oxide heterostructure photocatalyst.

[0060] The tungsten disulfide / zinc thioindate heterostructure photocatalyst prepared in Example 4 has a loading mass ratio of 12% for the tungsten disulfide nanosheets, and an appropriate amount of tungsten disulfide nanosheets grow on the surface of the zinc thioindate nanoflowers. Compared with the single-structure zinc thioindate, the appropriate amount of tungsten disulfide nanosheets in the tungsten disulfide / zinc thioindate heterostructure photocatalyst changes the color of the photocatalyst from yellow to slightly darker gray than Example 3. The UV-visible spectrophotometer proves that its light absorption capacity is enhanced, the visible light absorption limit is expanded, the band gap value is reduced, and the utilization rate of sunlight is improved (such as Figure 2 ); At the same time, the specific surface area of ​​this sample is increased, which increases the active sites for photocatalytic hydrogen production (such as Figure 3 ); In addition, due to the excellent conductivity of 1T phase tungsten disulfide, the separation of photogenerated electrons and holes in all-sulfoindium zinc oxide is promoted, which is beneficial to the transport of carriers and enhances the photocatalytic performance of the catalyst. Compared with Examples 1, 2 and 3, the tungsten disulfide / all-sulfoindium zinc oxide heterostructure photocatalyst has improved light absorption capacity under ultraviolet visible light, increased specific surface area, and enhanced photocatalytic water decomposition hydrogen production performance under simulated sunlight (such as Figure 4 ).

[0061] Example 5

[0062] The preparation method of the tungsten disulfide / zinc indium thioate heterostructure photocatalyst with a loading mass ratio of 17% of tungsten disulfide nanosheets is as follows:

[0063] Step 1: Add 0.136g of zinc chloride and 0.586g of indium tetrachloride tetrahydrate to 60mL of ethanol solution (ethanol: water = 1:4) and stir for 60 minutes to prepare a first mixed solution, then add 0.601g of thioacetamide to the above solution and stir for 60min to prepare a second mixed solution. After the above treatment, the second mixed solution is transferred to a 100mL reactor, kept in a heating box at 180°C for 20h, and cooled naturally to room temperature after heating. Finally, the product is collected, cleaned, and dried to obtain yellow zinc persulfoindate.

[0064] Step 2: Add 0.793g of tungsten hexachloride and 1.503g of thioacetamide powder to 60mL of N,N-dimethylformamide solution and stir for 30min to fully mix to prepare the third mixed solution. After the above treatment, transfer the third mixed solution to a 100mL reactor and keep it in a heating box at 200℃ for 24h at a heating rate of 5℃ / min. After heating, cool it naturally to room temperature. Finally, collect, wash and dry the product to obtain tungsten disulfide.

[0065] Step 3: Add 17 mg of tungsten disulfide and 100 mg of zinc persulfide indium oxide powder to a mortar. Add 5 mL of n-hexane and grind to dryness, followed by adding 3 mL of ethanol and grinding to dryness. Finally, the composite was washed with deionized water and ethanol, and the washed precipitate was dried in a vacuum to prepare a tungsten disulfide / zinc persulfide indium oxide heterostructure photocatalyst.

[0066] In the tungsten disulfide / zinc indium thioate heterostructure photocatalyst prepared in Example 5, the loading mass ratio of tungsten disulfide nanosheets is 17%, and the excess tungsten disulfide nanosheets grow on the surface of the zinc indium thioate nanoflowers.

[0067] In comparison, the excess tungsten disulfide nanosheets in the tungsten disulfide / perthioindinate zinc heterostructure photocatalyst changed the color of the photocatalyst from yellow to slightly darker gray than that of Example 4. The UV-visible spectrophotometer proved that its light absorption capacity was enhanced, the visible light absorption limit was expanded, the band gap value was reduced, and the utilization rate of sunlight was improved (such as Figure 2 ); Compared with Examples 1, 2, 3 and 4, the excess tungsten disulfide will cover the all-sulfoindium zinc nanoflowers, reducing the effective surface active sites, hindering the contact with water, and blocking the incident light, producing a shielding effect, and the specific surface area of ​​this sample is reduced (such as Figure 3 ), which reduces the catalytic activity of the catalyst. The light absorption capacity of the tungsten disulfide / perthioindium zinc heterostructure photocatalyst under ultraviolet visible light is improved, but due to the shielding effect, the photocatalytic decomposition of water to produce hydrogen under simulated sunlight is reduced (such as Figure 4 ).

[0068] Depend on Figure 2 Comparing the UV-visible absorption spectra of the tungsten disulfide / zinc indium thioate heterostructure photocatalysts prepared in Examples 1, 2, 3, 4 and 5, it can be seen that as the tungsten disulfide loading mass ratio increases, the band gap value decreases and the light absorption capacity of the heterostructure photocatalyst increases.

[0069] Depend on Figure 3 Comparing the specific surface areas of the tungsten disulfide / zinc indium thioate heterostructure photocatalysts prepared in Examples 1, 2, 3, 4 and 5, it can be seen that with zinc indium thioate as the matrix, as the tungsten disulfide loading mass ratio increases from 2 to 12%, the specific surface area of ​​the heterostructure photocatalyst increases continuously, but when the loading mass ratio increases to 17%, the specific surface area of ​​the heterostructure photocatalyst decreases. Therefore, the optimal loading mass ratio of the tungsten disulfide / zinc indium thioate heterostructure photocatalyst is 12%.

[0070] Depend on Figure 4Comparison of the photocatalytic decomposition of water and hydrogen production performance of the tungsten disulfide / zinc persulfoindium acid heterostructure photocatalysts prepared in Examples 1, 2, 3, 4 and 5 under simulated sunlight irradiation shows that, with zinc persulfoindium acid as the matrix, as the tungsten disulfide loading mass ratio increases from 2 to 12%, the photocatalytic decomposition of water and hydrogen production performance of the heterostructure photocatalyst increases continuously, but when the loading mass ratio increases to 17%, the photocatalytic decomposition of water and hydrogen production performance of the heterostructure photocatalyst decreases. Therefore, the optimal loading mass ratio of the tungsten disulfide / zinc persulfoindium acid heterostructure photocatalyst is 12%.

[0071] Test Example 1 Photocatalytic hydrogen production performance test

[0072] The products of Examples 1-5 were used as photocatalysts. The irradiation light source used was a 300 W Xe arc lamp (CELHXF300, Beijing Zhongjiao Jinyuan Co., Ltd.) equipped with an AM-1.5 filter, and the focusing intensity was 460.17 W m -2 , light receiving area (A R ) is about 1.59×10 −3 m 2 Specifically, 10 mg of the photocatalyst was dispersed in an external irradiation type photoreactor (100 mL quartz glass) containing 50 mL of lactic acid aqueous solution (lactic acid: water = 10 mL: 40 mL) and heated under N 2 The photocatalytic water decomposition experiment was carried out for 4 hours under a gas atmosphere. The evolved gas was analyzed using a gas chromatograph (Techcomp GC-7920) equipped with a thermal conductivity detector (TCD).

[0073] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A metal sulfur-based semiconductor photocatalyst, It is characterized in that The catalyst is a tungsten disulfide nanosheet layered on the surface of the zinc indium thioate nanoflower, and a two-dimensional / two-dimensional structure formed by the tungsten disulfide nanosheet and the zinc indium thioate; the tungsten sulfide is composed of a 1T and 2H mixed phase, with the 1T phase being the main phase; the 1T phase accounts for 75-76%, and the 2H phase accounts for 24-25%; the preparation method comprises: Adding zinc chloride and indium tetrachloride tetrahydrate powder to an ethanol / water mixture, stirring and fully dissolving to prepare a first mixture; Adding thioacetamide powder to the first mixed solution, stirring and mixing thoroughly to prepare a second mixed solution; The second mixed solution is transferred to a reactor for reaction, and the product is calcined to obtain a zinc persulfide indium acid photocatalyst; Adding tungsten hexachloride and thioacetamide powder to the N,N-dimethylformamide solution, stirring and mixing thoroughly to prepare a third mixed solution; The third mixed solution is transferred to a reactor for hydrothermal reaction, and the product is calcined to obtain a tungsten disulfide nanosheet photocatalyst; the temperature of the hydrothermal reaction is 190-220°C; the heating rate of the hydrothermal reaction is 4-6°C / min; and the hydrothermal reaction insulation time is 20-36h; Add zinc indium thioate and tungsten disulfide nanosheets into a mortar, add n-hexane and ethanol and grind evenly to obtain a tungsten disulfide / zinc indium thioate heterostructure photocatalyst.

2. According to the metal sulfur-based semiconductor photocatalyst of claim 1, the mass ratio of tungsten disulfide to zinc indium thioate is 2-17:

100.

3. According to the metal sulfur-based semiconductor photocatalyst of claim 2, the mass ratio of tungsten disulfide to zinc indium thioate is 12:

100.

4. The metal-sulfur-based semiconductor photocatalyst according to claim 1, It is characterized in that The temperature of the hydrothermal reaction is 200° C.; the heating rate of the hydrothermal reaction is 5° C. / min; and the holding time of the hydrothermal reaction is 24 h.

5. Use of the metal-sulfur-based semiconductor photocatalyst as claimed in any one of claims 1 to 4 in photocatalytic decomposition of water to produce hydrogen.