A kind of biodegradable plant cellulose glitter powder
Through the activation treatment and blending technology of plant fiber powder, a glans powder coating with high brightness, mild and acid-base resistance is formed, which solves the problems of insufficient brightness and poor tolerance of existing glans powder, and achieves a wider range of Application.
Patent Information
- Application Number
- CN202410657682.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-26
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-05-26
AI Technical Summary
The existing glitter powder has insufficient brightness, poor temperature and corrosion resistance, which limits its application range.
By activating the plant fiber powder and blending it with 1-butyl-3-methylimidazole chloride, polybutylene succinate and coupling agent, it forms a degradable, gentle and acid-resistant environment. Alkaline properties coating.
It improves the degradability, wear resistance and chemical corrosion resistance of the green onion powder, and enhances its stable performance in harsh environments.
Smart Images

Figure CN118515900B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of glitter powder, in particular to degradable plant cellulose glitter powder. Background Art
[0002] Glitter powder is a kind of glitter powder made by electroplating and coating PET, PVC, OPP metal aluminum film materials with different thicknesses and high brightness, and then precisely cut. Glitter powder has various shapes, such as quadrilateral, hexagon, rectangle, etc. Glitter powder has rich colors, including laser silver, laser gold, laser color, silver, gold, color and other fantasy color series. Each color series is added with a surface protective layer, with bright color, and has certain resistance to mildly corrosive chemicals of climate and temperature and temperature resistance.
[0003] Cellulose is a macromolecular polysaccharide composed of D-glucose with β-1,4-glycosidic bonds. Adjacent glucose rings in the crystal region are inverted, and the hydrogen atoms and hydroxyl groups in the sugar rings are distributed on both sides of the sugar ring plane. Due to the aggregated structural characteristics of natural cellulose and the presence of many hydrogen bonds between and within molecules and a high degree of crystallinity, it cannot be dissolved in water and general organic and inorganic solvents, lacks thermoplasticity, and has poor chemical corrosion resistance and strength, which is extremely unfavorable for its molding, processing and application, resulting in many restrictions on its application.
[0004] The glitter powder formed by using PET sheet as substrate and cellulose as coating on the substrate has the following disadvantages:
[0005] Lack of brilliance: Cellulose coatings may be less reflective and less bright than metallic aluminum films, making the glitter effect less intense.
[0006] Poor temperature and corrosion resistance: The temperature and corrosion resistance of cellulose coating may not be as good as that of metallic aluminum film, which may cause the performance of glitter powder to deteriorate in harsh environments. Summary of the invention
[0007] In order to overcome the shortcomings of the prior art, the degradable plant cellulose-based glitter powder described in this application is obtained by activating the plant fiber powder, then dissolving 1-butyl-3-methylimidazole chloride, blending it with coupling agent and polybutylene succinate, to obtain a degradable coating not only has degradable function, but also has good temperature resistance and acid and alkali resistance.
[0008] The technical solution adopted by the present invention to solve its technical problem is:
[0009] A degradable plant cellulose glitter powder comprises a substrate sheet and a degradable coating attached to the substrate sheet.
[0010] The degradable coating comprises the following raw materials in parts by weight:
[0011] 72-102 parts of cellulose composite, 1-3 parts of grafting agent, 5-10 parts of pigment;
[0012] The cellulose composite comprises the following raw materials in parts by weight:
[0013] 40-50 parts of plant fiber powder, 3-5 parts of diphenylmethane diisocyanate, 20-30 parts of polybutylene succinate, 5-10 parts of plasticizer, 3-5 parts of coupling agent, 1-2 parts of antioxidant;
[0014] The preparation method of the cellulose composite comprises the following steps:
[0015] The plant fiber powder is activated, and then the plasticizer and diphenylmethane diisocyanate are added for hydrophobic treatment to obtain a mixture; the mixture is added with polybutylene succinate, coupling agent, and antioxidant, and blended and extruded to obtain a cellulose composite.
[0016] In the application, diphenylmethane diisocyanate is used as a crosslinking agent, which can react with the hydroxyl groups in cellulose to form stable chemical bonds, thereby enhancing the mechanical strength and chemical resistance of the coating.
[0017] Polybutylene succinate has excellent mechanical properties, including high strength and good toughness. Adding polybutylene succinate to cellulose composites can significantly improve the mechanical properties of the final product, making it more resistant to wear and tear. Polybutylene succinate has good thermal stability and can remain stable at higher temperatures. This allows cellulose composites to withstand higher temperatures during processing, such as extrusion and coating, without affecting product quality due to thermal decomposition; the addition of polybutylene succinate can improve the processing properties of cellulose composites, including fluidity and processing temperature range, making cellulose composites easier to process and shape in industrial production;
[0018] At the same time, polybutylene succinate is a biodegradable polyester that can be degraded within a certain period of time under the action of microorganisms. Therefore, the addition of polybutylene succinate helps to improve the biodegradability of cellulose composites and meets environmental protection requirements; polybutylene succinate has good chemical corrosion resistance and can improve the tolerance of cellulose composites to chemical substances such as acids and alkalis, thereby improving the chemical resistance of the coating.
[0019] Furthermore, the plant fiber powder is any one of corn straw powder, wheat straw powder and rice straw powder.
[0020] Further, the plant fiber powder is activated to soak the plant fiber powder in an alkali solution and react at 50-60°C for 1-2 hours. After the reaction is completed, it is filtered, washed and dried to obtain the activated plant fiber powder.
[0021] Furthermore, the process of hydrophobic treatment is as follows: fully mix the activated plant fiber powder, plasticizer, diphenylmethane diisocyanate, and triethylamine, react at 30-40°C for 3-4 hours, filter and dry to obtain isocyanate cellulose. Diphenylmethane diisocyanate reacts with the hydroxyl groups on the surface of cellulose to hydrophobically modify it, thereby improving the compatibility of cellulose with polybutylene succinate. At the same time, adding a plasticizer can reduce the processing difficulty of the plant fiber powder.
[0022] Further, the plasticizer is 1-butyl-3-methylimidazole chloride. In this application, the addition of plasticizers can improve the flexibility and processing properties of the cellulose composite and reduce its brittleness, thereby improving the adhesion and temperature resistance of the coating.
[0023] Further, the coupling agent is a silane coupling agent, and silane coupling agent KH550 can be specifically selected. In this application, the coupling agent can promote the adhesion between the cellulose composite and the substrate sheet, and improve the adhesion and wear resistance of the coating.
[0024] Further, the antioxidant is a hydroxylamine-based antioxidant. In this application, the addition of antioxidants can prevent thermal oxidation and degradation of the material during processing and use, and extend the service life of the product.
[0025] Further, the grafting agent is methylene succinic acid. In this application, the grafting agent connects the cellulose composite and pigment through chemical bonding through its chemical properties to form a stable graft copolymer, which can enhance the adhesion between the coating material and the substrate sheet, so that the coating adheres more firmly to the substrate sheet, thereby improving the wear resistance and overall stability of the glaze powder.
[0026] Further, the pigments include any or any of iron oxide red, iron oxide black, titanium dioxide yellow, zinc chromium yellow, lead chromium green, zinc white, iron blue, and cobalt blue. In this application, pigments are the main source of the color of glitter pink. By adding different types and proportions of pigments, glitter powders of different colors and tones can be prepared to meet the decoration and beautification needs in different application scenarios.
[0027] Further, the base sheet is a base sheet obtained by blending and extruding polyethylene terephthalate and polybutylene succinate. In this application, the base sheet provides the basic shape and size of the green onion powder, providing a basis for adhesion for coatings and pigments, and the base sheet also uses a degradable material, so that the green onion powder has better environmental protection properties.
[0028] In the substrate, polybutylene succinate (PBST) is one of the raw materials for the substrate sheet and has the following uses:
[0029] Forming the main structure of the substrate: PBST, as a polymer material, is the main component of the substrate sheet. It provides the basic physical form and chemical properties for the substrate.
[0030] Improve the mechanical properties of the substrate: PBST has good mechanical properties, such as high strength, toughness and wear resistance. Using PBST in the substrate sheet helps to improve its overall mechanical strength and durability.
[0031] Enhance the thermal stability of the substrate: PBST has a high melting point and good thermal stability. It can withstand high temperatures during processing without thermal decomposition, ensuring the stability of the substrate sheet in the production process.
[0032] Improve the processing properties of the substrate: The addition of PBST can improve the processing properties of the substrate, such as extrusion moldability, making the production of substrate sheets more efficient and controllable.
[0033] Providing substrate degradability: As a biodegradable material, the addition of PBST helps to improve the environmental friendliness of the substrate sheet, which meets the current demand for sustainable development and environmentally friendly materials.
[0034] Enhance the adhesion between coating and substrate: The good compatibility between PBST and cellulose composite helps to improve the bonding strength between coating and substrate, ensuring the uniformity and adhesion of coating.
[0035] Improve the chemical stability of the substrate: PBST has good chemical corrosion resistance and can resist the erosion of a variety of chemical substances, thereby improving the chemical resistance of the substrate sheet.
[0036] Furthermore, the preparation method of glitter powder comprises the following steps:
[0037] 1) Preparation of substrate sheet
[0038] 2) Cellulose complex
[0039] 3) Preparation of coating slurry
[0040] After mixing the cellulose composite, grafting agent and pigment, a coating slurry is obtained.
[0041] 4) Coating
[0042] The substrate sheet is coated with a printed coating slurry; after drying, the sheet is cut to obtain glitter powder.
[0043] In the above technical scheme, the plant fiber powder is activated through activation treatment, which increases its reactivity and enables it to be better combined with other components; through the process of co-extrusion, the various components in the cellulose composite are evenly mixed and tightly combined to form a functional material with stable structure and excellent performance; the polybutylene succinate and other additives in the cellulose composite give the coating good temperature resistance and acid and alkali resistance, so that the glitter powder can maintain stable performance in different environments. Therefore, the prepared cellulose composite is used to prepare the degradable coating of glitter powder. The degradable coating prepared by mixing the cellulose composite, the grafting agent and the pigment together constitutes a functional layer that is not only degradable, but also has good temperature resistance and acid and alkali resistance.
[0044] The beneficial effects of the present invention are:
[0045] 1. The glitter powder described in the present application has good degradability by preparing a degradable substrate sheet and attaching a degradable coating on the substrate sheet.
[0046] 2. The green onion powder described in this application is activated by activate the plant fiber powder, then dissolved by 1-butyl-3-methylimidazole chloride, and blended by coupling agent and blending of polybutylene succinate, and extruded by blending and extruding, to obtain a degradable coating that not only has degradable function, but also has good temperature resistance and acid and alkali resistance.
[0047] 3. The glans powder described in this application can adhere well to the base sheet during the coating process by grafting agent, and the coating and the base sheet are well combined, and have good wear resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] The present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0049] Figure 1 A process flow chart of the method for preparing glitter powder described in this application. DETAILED DESCRIPTION
[0050] In order to facilitate the understanding of those skilled in the art, the present invention is further described below in conjunction with embodiments, and the contents mentioned in the implementation modes are not intended to limit the present invention.
[0051] As used herein, "and / or" includes the term of any and all combinations of one or more associated listed items. The terms used herein are only used to describe specific embodiments and are not intended to limit the present invention. As used herein, the singular forms "a", "an", "an" and "the" are also intended to include the plural forms, unless the context clearly indicates otherwise. It is further understood that "including", when used in this specification, specifies the stated features, integers, steps, operations, elements and / or compositions, but does not exclude the existence or addition of one or more other features, integers, steps, operations, elements, compositions and / or combinations thereof.
[0052] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning generally understood by those of ordinary skill in the art to which the invention belongs. Further understanding, terms, such as defined in common dictionaries, explain consistent with their meaning in the context of the relevant field and are not idealized or overly formal, unless explicitly so defined here.
[0053] The exemplary invention described herein may appropriately lack any one or more element limitations that are not specifically disclosed herein. Therefore, the terms "comprise", "include", "contain", etc. should be understood broadly and non-restrictively. In addition, the terminology used herein is used as a description, not a limitation, and it is unintentional to use these terminology expressions that do not include any equivalent characteristics, but only describe some of their characteristics, but various modifications are possible within the scope of the present invention according to the rights. Therefore, although the present invention has been specifically disclosed by preferred embodiments and optional features, the modifications disclosed herein to embody the changes of the present invention may be recorded by those skilled in the art, and such modifications and changes will be considered to be within the scope of the present invention.
[0054] Some of the raw materials come from:
[0055] Polybutylene succinate, CAS No. 79917-90-1;
[0056] 1-Butyl-3-methylimidazolium chloride, CAS No.: 79917-90-1;
[0057] Hydroxylamine antioxidant, antioxidant 420;
[0058] Polyethylene terephthalate, CAS No.: 25038-59-9;
[0059] Silane coupling agent, KH550 is used.
[0060] Example 1
[0061] A degradable plant cellulose glitter powder comprises a substrate sheet and a degradable coating attached to the substrate sheet.
[0062] The degradable coating comprises the following raw materials in parts by weight:
[0063] 72 parts of cellulose composite, 1 part of grafting agent (methylene succinic acid), 5 parts of pigment (iron oxide red);
[0064] The preparation method of glitter powder comprises the following steps:
[0065] 1) Preparation of substrate sheet
[0066] Polyethylene terephthalate and polybutylene succinate were placed in a vacuum drying box, and dried at 60°C and 80°C. Then, premixed according to a mass ratio of 1:1 and added to a single screw extruder, extrusion and molding, to obtain a base sheet. The temperature of each section of the single screw extruder is set to 160℃-175℃-175℃-165℃, the screw speed is 40r / min, and the feed volume is 4kg / h.
[0067] 2) Cellulose complex
[0068] 40 parts of plant fiber powder (corn straw powder) were soaked in an alkali solution (a sodium hydroxide solution with a mass concentration of 20%), and reacted at 50°C for 2 hours. After the reaction was completed, it was filtered, washed and dried to obtain the activated plant fiber powder.
[0069] The activated plant fiber powder, 5 parts of plasticizer, 3 parts of diphenylmethane diisocyanate, and 0.02 parts of triethylamine were thoroughly mixed, and then reacted at 30°C for 4 hours, then filtered and dried to obtain isocyanated cellulose.
[0070] The isocyanated cellulose, 20 parts of polybutylene succinate, 3 parts of coupling agent, and 1 part of antioxidant were mixed in the mixer, and then melted and extruded at 160°C through a twin-screw extruder to obtain a cellulose composite.
[0071] 3) Preparation of coating slurry
[0072] The cellulose composite in step 2), 1 part of the grafting agent, 5 parts of the pigment and 150 parts of DMF are mixed evenly in a mixer to obtain a coating slurry.
[0073] 4) Coating
[0074] The coating slurry is applied on the substrate sheet with a scraper and dried at 90° C. After drying, it is cut to obtain glitter powder.
[0075] Example 2
[0076] A degradable plant cellulose glitter powder comprises a substrate sheet and a degradable coating attached to the substrate sheet.
[0077] The degradable coating comprises the following raw materials in parts by weight:
[0078] 102 parts of cellulose composite, 3 parts of grafting agent (methylene succinic acid), 10 parts of pigment (iron oxide red);
[0079] The preparation method of glitter powder comprises the following steps:
[0080] 1) Preparation of substrate sheet
[0081] Polyethylene terephthalate and polybutylene succinate were placed in a vacuum drying box, and dried at 60°C and 80°C. Then, premixed according to a mass ratio of 1:1 and added to a single screw extruder, extrusion and molding, to obtain a base sheet. The temperature of each section of the single screw extruder is set to 160℃-175℃-175℃-165℃, the screw speed is 40r / min, and the feed volume is 4kg / h.
[0082] 2) Cellulose complex
[0083] 50 parts of the plant fiber powder were soaked in an alkali solution (a sodium hydroxide solution with a mass concentration of 20%) and reacted at 60°C for 1 h; after the reaction was completed, it was filtered, washed and dried to obtain the activated plant fiber powder.
[0084] The activated plant fiber powder, 10 parts of plasticizer, 5 parts of diphenylmethane diisocyanate, and 0.02 parts of triethylamine were thoroughly mixed, and then reacted at 40°C for 4 hours, then filtered and dried to obtain isocyanated cellulose.
[0085] The isocyanated cellulose, 30 parts of polybutylene succinate, 5 parts of coupling agent, and 2 parts of antioxidant were mixed in the mixer, and then melted and extruded at 160°C through a twin-screw extruder to obtain a cellulose composite.
[0086] 3) Preparation of coating slurry
[0087] The cellulose composite in step 2), 2 parts of the grafting agent, 8 parts of the pigment and 150 parts of DMF were mixed evenly in a mixer to obtain a coating slurry.
[0088] 4) Coating
[0089] The coating slurry is applied on the substrate sheet with a scraper and dried at 95° C. After drying, it is cut to obtain glitter powder.
[0090] Example 3
[0091] A degradable plant cellulose glitter powder comprises a substrate sheet and a degradable coating attached to the substrate sheet.
[0092] The degradable coating comprises the following raw materials in parts by weight:
[0093] 78 parts of cellulose composite, 2 parts of grafting agent (methylene succinic acid), 6 parts of pigment (iron oxide red);
[0094] The preparation method of glitter powder comprises the following steps:
[0095] 1) Preparation of substrate sheet
[0096] Polyethylene terephthalate and polybutylene succinate were placed in a vacuum drying box, and dried at 60°C and 80°C. Then, premixed according to a mass ratio of 1:1 and added to a single screw extruder, extrusion and molding, to obtain a base sheet. The temperature of each section of the single screw extruder is set to 160℃-175℃-175℃-165℃, the screw speed is 40r / min, and the feed volume is 4kg / h.
[0097] 2) Cellulose complex
[0098] 42 parts of plant fiber powder (corn straw powder) were soaked in an alkali solution (potassium hydroxide solution with a mass concentration of 20%), and reacted at 60°C for 1 h; after the reaction was completed, it was filtered, washed and dried to obtain the activated plant fiber powder.
[0099] The activated plant fiber powder, 6 parts of plasticizer, 4 parts of diphenylmethane diisocyanate, and 0.02 parts of triethylamine were thoroughly mixed, and then reacted at 40°C for 3 hours, then filtered and dried to obtain isocyanated cellulose.
[0100] The isocyanated cellulose, 22 parts of polybutylene succinate, 3 parts of coupling agent, and 1 part of antioxidant were mixed in the mixer, and then melted and extruded at 160°C through a twin-screw extruder to obtain a cellulose composite.
[0101] 3) Preparation of coating slurry
[0102] The cellulose composite in step 2), 2 parts of the grafting agent, 6 parts of the pigment and 150 parts of DMF were mixed evenly in a mixer to obtain a coating slurry.
[0103] 4) Coating
[0104] The coating slurry is applied on the substrate sheet with a scraper and dried at 90° C. After drying, it is cut to obtain glitter powder.
[0105] Example 4
[0106] A degradable plant cellulose glitter powder comprises a substrate sheet and a degradable coating attached to the substrate sheet.
[0107] The degradable coating comprises the following raw materials in parts by weight:
[0108] 88 parts of cellulose composite, 2 parts of grafting agent (methylene succinic acid), 8 parts of pigment (iron oxide red);
[0109] The preparation method of glitter powder comprises the following steps:
[0110] 1) Preparation of substrate sheet
[0111] Polyethylene terephthalate and polybutylene succinate were placed in a vacuum drying box, and dried at 60°C and 80°C. Then, premixed according to a mass ratio of 1:1 and added to a single screw extruder, extrusion and molding, to obtain a base sheet. The temperature of each section of the single screw extruder is set to 160℃-175℃-175℃-165℃, the screw speed is 40r / min, and the feed volume is 4kg / h.
[0112] 2) Cellulose complex
[0113] 45 parts of plant fiber powder (corn straw powder) were soaked in an alkali solution (a sodium hydroxide solution with a mass concentration of 20%), and reacted at 60°C for 1 h; after the reaction was completed, it was filtered, washed and dried to obtain the activated plant fiber powder.
[0114] The activated plant fiber powder, 8 parts of plasticizer, 4 parts of diphenylmethane diisocyanate, and 0.02 parts of triethylamine were thoroughly mixed, and the reaction was carried out at 30°C for 3.5 hours, then filtered and dried to obtain isocyanated cellulose.
[0115] The isocyanated cellulose, 25 parts of polybutylene succinate, 4 parts of coupling agent, and 2 parts of antioxidant were mixed in the mixer, and then melted and extruded at 160°C through a twin-screw extruder to obtain a cellulose composite.
[0116] 3) Preparation of coating slurry
[0117] The cellulose composite in step 2), 2 parts of the grafting agent, 8 parts of the pigment and 150 parts of DMF were mixed evenly in a mixer to obtain a coating slurry.
[0118] 4) Coating
[0119] The coating slurry is applied on the substrate sheet with a scraper and dried at 95° C. After drying, it is cut to obtain glitter powder.
[0120] Example 5
[0121] A degradable plant cellulose glitter powder comprises a substrate sheet and a degradable coating attached to the substrate sheet.
[0122] The degradable coating comprises the following raw materials in parts by weight:
[0123] 92 parts of cellulose composite, 1 part of grafting agent (methylene succinic acid), 8 parts of pigment (iron oxide red);
[0124] The preparation method of glitter powder comprises the following steps:
[0125] 1) Preparation of substrate sheet
[0126] Polyethylene terephthalate and polybutylene succinate were placed in a vacuum drying box, and dried at 60°C and 80°C. Then, premixed according to a mass ratio of 1:1 and added to a single screw extruder, extrusion and molding, to obtain a base sheet. The temperature of each section of the single screw extruder is set to 160℃-175℃-175℃-165℃, the screw speed is 40r / min, and the feed volume is 4kg / h.
[0127] 2) Cellulose complex
[0128] 48 parts of plant fiber powder (corn straw powder) were soaked in an alkali solution (a sodium hydroxide solution with a mass concentration of 20%), and reacted at 50°C for 2 hours. After the reaction was completed, it was filtered, washed and dried to obtain the activated plant fiber powder.
[0129] The activated plant fiber powder, 8 parts of plasticizer, 3 parts of diphenylmethane diisocyanate, and 0.02 parts of triethylamine were thoroughly mixed, and the reaction was carried out at 40°C for 4 hours, then filtered and dried to obtain isocyanated cellulose.
[0130] The isocyanated cellulose, 28 parts of polybutylene succinate, 3 parts of coupling agent, and 2 parts of antioxidant were mixed in the mixer, and then melted and extruded at 160°C through a twin-screw extruder to obtain a cellulose composite.
[0131] 3) Preparation of coating slurry
[0132] The cellulose composite in step 2), 1 part of the grafting agent, 8 parts of the pigment and 150 parts of DMF were mixed evenly in a mixer to obtain a coating slurry.
[0133] 4) Coating
[0134] The coating slurry is applied on the substrate sheet with a scraper and dried at 90° C. After drying, it is cut to obtain glitter powder.
[0135] Example 6
[0136] A degradable plant cellulose glitter powder comprises a substrate sheet and a degradable coating attached to the substrate sheet.
[0137] The degradable coating comprises the following raw materials in parts by weight:
[0138] 81 parts of cellulose composite, 1 part of grafting agent (methylene succinic acid), 5 parts of pigment (iron oxide red);
[0139] The preparation method of glitter powder comprises the following steps:
[0140] 1) Preparation of substrate sheet
[0141] Polyethylene terephthalate and polybutylene succinate were placed in a vacuum drying box, and dried at 60°C and 80°C. Then, premixed according to a mass ratio of 1:1 and added to a single screw extruder, extrusion and molding, to obtain a base sheet. The temperature of each section of the single screw extruder is set to 160℃-175℃-175℃-165℃, the screw speed is 40r / min, and the feed volume is 4kg / h.
[0142] 2) Cellulose complex
[0143] 44 parts of plant fiber powder (corn straw powder) were soaked in an alkali solution (a sodium hydroxide solution with a mass concentration of 20%), and reacted at 50°C for 2 hours. After the reaction was completed, it was filtered, washed and dried to obtain the activated plant fiber powder.
[0144] The activated plant fiber powder, 7 parts of plasticizer, 4 parts of diphenylmethane diisocyanate, and 0.02 parts of triethylamine were thoroughly mixed, and then reacted at 30°C for 4 hours, then filtered and dried to obtain isocyanated cellulose.
[0145] The isocyanated cellulose, 22 parts of polybutylene succinate, 3 parts of coupling agent, and 1 part of antioxidant were mixed in the mixer, and then melted and extruded at 160°C through a twin-screw extruder to obtain a cellulose composite.
[0146] 3) Preparation of coating slurry
[0147] The cellulose composite in step 2), 1 part of the grafting agent, 5 parts of the pigment and 150 parts of DMF are mixed evenly in a mixer to obtain a coating slurry.
[0148] 4) Coating
[0149] The coating slurry is applied on the substrate sheet with a scraper and dried at 90° C. After drying, it is cut to obtain glitter powder.
[0150] Comparative Example 1
[0151] A glitter powder, comprising a substrate sheet and a cellulose layer attached to the substrate sheet,
[0152] The cellulose layer comprises the following raw materials in parts by weight:
[0153] 72 parts of activated plant fiber powder, 1 part of grafting agent (methylene succinic acid), 5 parts of pigment (red iron oxide);
[0154] The preparation method of glitter powder comprises the following steps:
[0155] 1) Preparation of substrate sheet
[0156] Polyethylene terephthalate and polybutylene succinate were placed in a vacuum drying box, and dried at 60°C and 80°C. Then, premixed according to a mass ratio of 1:1 and added to a single screw extruder, extrusion and molding, to obtain a base sheet. The temperature of each section of the single screw extruder is set to 160℃-175℃-175℃-165℃, the screw speed is 40r / min, and the feed volume is 4kg / h.
[0157] 2) Cellulose complex
[0158] 72 parts of plant fiber powder (corn straw powder) were soaked in an alkali solution (a sodium hydroxide solution with a mass concentration of 20%), and reacted at 50°C for 2 hours. After the reaction was completed, it was filtered, washed and dried to obtain the activated plant fiber powder.
[0159] 3) Preparation of coating slurry
[0160] The activated plant fiber powder in step 2), 1 part of a grafting agent, 5 parts of a pigment, and 150 parts of DMF are uniformly mixed in a mixer to obtain a coating slurry.
[0161] 4) Coating
[0162] The coating slurry is applied on the substrate sheet with a scraper and dried at 90° C. After drying, it is cut to obtain glitter powder.
[0163] Comparative Example 2
[0164] A degradable plant cellulose glitter powder comprises a substrate sheet and a degradable coating attached to the substrate sheet.
[0165] The degradable coating comprises the following raw materials in parts by weight:
[0166] 72 parts of cellulose composite, 5 parts of pigment (iron oxide red);
[0167] The preparation method of glitter powder comprises the following steps:
[0168] 1) Preparation of substrate sheet
[0169] Polyethylene terephthalate and polybutylene succinate were placed in a vacuum drying box, and dried at 60°C and 80°C. Then, premixed according to a mass ratio of 1:1 and added to a single screw extruder, extrusion and molding, to obtain a base sheet. The temperature of each section of the single screw extruder is set to 160℃-175℃-175℃-165℃, the screw speed is 40r / min, and the feed volume is 4kg / h.
[0170] 2) Cellulose complex
[0171] 40 parts of plant fiber powder (corn straw powder) were soaked in an alkali solution (a sodium hydroxide solution with a mass concentration of 20%), and reacted at 50°C for 2 hours. After the reaction was completed, it was filtered, washed and dried to obtain the activated plant fiber powder.
[0172] The activated plant fiber powder, 5 parts of plasticizer, 3 parts of diphenylmethane diisocyanate, and 0.02 parts of triethylamine were thoroughly mixed, and then reacted at 30°C for 4 hours, then filtered and dried to obtain isocyanated cellulose.
[0173] The isocyanated cellulose, 20 parts of polybutylene succinate, 3 parts of coupling agent, and 1 part of antioxidant were mixed in the mixer, and then melted and extruded at 160°C through a twin-screw extruder to obtain a cellulose composite.
[0174] 3) Preparation of coating slurry
[0175] The cellulose composite in step 2), 5 parts of pigment and 150 parts of DMF are mixed evenly in a mixer to obtain a coating slurry.
[0176] 4) Coating
[0177] The coating slurry is applied on the substrate sheet with a scraper and dried at 90° C. After drying, it is cut to obtain glitter powder.
[0178] Comparative Example 3
[0179] A degradable plant cellulose glitter powder comprises a substrate sheet and a degradable coating attached to the substrate sheet.
[0180] The degradable coating comprises the following raw materials in parts by weight:
[0181] 72 parts of cellulose composite, 1 part of grafting agent (methylene succinic acid), 5 parts of pigment (iron oxide red);
[0182] The preparation method of glitter powder comprises the following steps:
[0183] 1) Preparation of substrate sheet
[0184] Polybutylene succinate was placed in a vacuum drying box and dried at 80°C. Then, a single screw extruder was added to extrude and molded to obtain a substrate sheet. The temperature of each section of the single screw extruder is set to 160℃-175℃-175℃-165℃, the screw speed is 40r / min, and the feed volume is 4kg / h.
[0185] 2) Cellulose complex
[0186] 40 parts of plant fiber powder (corn straw powder) were soaked in an alkali solution (a sodium hydroxide solution with a mass concentration of 20%), and reacted at 50°C for 2 hours. After the reaction was completed, it was filtered, washed and dried to obtain the activated plant fiber powder.
[0187] The activated plant fiber powder, 5 parts of plasticizer, 3 parts of diphenylmethane diisocyanate, and 0.02 parts of triethylamine were thoroughly mixed, and then reacted at 30°C for 4 hours, then filtered and dried to obtain isocyanated cellulose.
[0188] The isocyanated cellulose, 20 parts of polybutylene succinate, 3 parts of coupling agent, and 1 part of antioxidant were mixed in the mixer, and then melted and extruded at 160°C through a twin-screw extruder to obtain a cellulose composite.
[0189] 3) Preparation of coating slurry
[0190] The cellulose composite in step 2), 1 part of the grafting agent, 5 parts of the pigment and 150 parts of DMF are mixed evenly in a mixer to obtain a coating slurry.
[0191] 4) Coating
[0192] The coating slurry is applied on the substrate sheet with a scraper and dried at 90° C. After drying, it is cut to obtain glitter powder.
[0193] Comparative Example 4
[0194] A degradable plant cellulose glitter powder comprises a substrate sheet and a degradable coating attached to the substrate sheet.
[0195] The degradable coating comprises the following raw materials in parts by weight:
[0196] 72 parts of cellulose composite, 1 part of grafting agent (methylene succinic acid), 5 parts of pigment (iron oxide red);
[0197] The preparation method of glitter powder comprises the following steps:
[0198] 1) Preparation of substrate sheet
[0199] Polyethylene terephthalate and polybutylene succinate were placed in a vacuum drying box, and dried at 60°C and 80°C. Then, premixed according to a mass ratio of 1:1 and added to a single screw extruder, extrusion and molding, to obtain a base sheet. The temperature of each section of the single screw extruder is set to 160℃-175℃-175℃-165℃, the screw speed is 40r / min, and the feed volume is 4kg / h.
[0200] 2) Cellulose complex
[0201] 60 parts of plant fiber powder (corn straw powder) were soaked in an alkali solution (a sodium hydroxide solution with a mass concentration of 20%), and reacted at 50°C for 2 hours. After the reaction was completed, it was filtered, washed and dried to obtain the activated plant fiber powder.
[0202] The activated plant fiber powder, 5 parts of plasticizer, 3 parts of diphenylmethane diisocyanate, and 0.02 parts of triethylamine were thoroughly mixed, and then reacted at 30°C for 4 hours, then filtered and dried to obtain isocyanated cellulose.
[0203] Isocyanate-modified cellulose, 3 parts of a coupling agent, and 1 part of an antioxidant are uniformly mixed in a mixer, and then melt-extruded at 160° C. through a twin-screw extruder to obtain a cellulose composite.
[0204] 3) Preparation of coating slurry
[0205] The cellulose composite in step 2), 1 part of the grafting agent, 5 parts of the pigment and 150 parts of DMF are mixed evenly in a mixer to obtain a coating slurry.
[0206] 4) Coating
[0207] The coating slurry is applied on the substrate sheet with a scraper and dried at 90° C. After drying, it is cut to obtain glitter powder.
[0208] Performance test: The glitter powder prepared in Examples 1-6 and Comparative Examples 1-4 was subjected to the following performance tests, and the test results are summarized in Table 1:
[0209] 1. Degradability. Ginger powder was soaked in an amylase buffer solution with a mass fraction of 5% (phosphate buffer solution with pH 5.5). Its degradability was characterized by testing its degradability for 30 days and 50 days.
[0210] 2. Alkali resistance: boil the glitter powder in a sodium hydroxide solution with a pH of 10 (maintained at 80°C) and observe the surface color. If there is no effect on the color quality, it is 0; if there is any effect on the color quality, it is 1.
[0211] 3. Temperature resistance. After placing the green onion powder at 180℃, 190℃ and 200℃ for 10 days, compare and observe whether it affects the color rendering; if there is no effect on the color rendering quality, it is 0, and if there is any effect on the color rendering, it is 1;
[0212] Table 1
[0213] 30-day weight loss rate (%) 50-day weight loss rate (%) Alkali resistance Temperature resistance Example 1 23 55 0 0 Example 2 21 52 0 0 Example 3 26 60 0 0 Example 4 22 54 0 0 Example 5 23 56 0 0 Example 6 25 58 0 0 Comparative Example 1 10 36 1 1 Comparative Example 2 18 49 1 1 Comparative Example 3 13 36 0 1 Comparative Example 4 5 21 0 1
[0214] From Table 1, it can be seen that the glitter powder prepared in Examples 1-6 has a weight loss rate of more than 21% in 30 days and a weight loss rate of more than 52% in 50 days in the degradability test, and has good alkali resistance and temperature resistance. From Comparative Examples 1, 2, 3, and 4, it can be seen that when the plant fiber powder is not coupled and blended, when no grafting agent is added, when polybutylene succinate is not added to the substrate, and when no cellulose composite is added to the cellulose composite, the weight loss rate in 30 days and the weight loss rate in 50 days are significantly reduced, and the alkali resistance or temperature resistance also shows a certain degree of reduction.
[0215] The raw materials or reagents used in the embodiments of the present invention and the comparative examples are all purchased from mainstream manufacturers in the market. Those without indicating the manufacturer or the concentration are all analytically pure raw materials or reagents that can be routinely obtained, as long as they can play the expected role, there is no particular restriction. The instruments and equipment such as the reactor and rotary evaporator used in the present embodiment are all purchased from major manufacturers in the market, as long as they can play the expected role, there is no particular restriction. If specific techniques or conditions are not indicated in the present embodiment, the techniques or conditions described in the literature in this area or according to the product specification are carried out.
[0216] The above-mentioned embodiments are preferred implementation solutions of the present invention. In addition, the present invention can be implemented in other ways, and any obvious replacements are within the protection scope of the present invention without departing from the inventive concept.
Claims
1. A degradable plant cellulose glitter powder, characterized in that: The invention comprises a substrate sheet and a degradable coating attached to the substrate sheet, The degradable coating comprises the following raw materials in parts by weight: 72-102 parts of cellulose composite, 1-3 parts of grafting agent, 5-10 parts of pigment; The cellulose composite comprises the following raw materials in parts by weight: 40-50 parts of plant fiber powder, 3-5 parts of diphenylmethane diisocyanate, 20-30 parts of polybutylene succinate, 5-10 parts of plasticizer, 3-5 parts of coupling agent, 1-2 parts of antioxidant; The preparation method of the cellulose composite comprises the following steps: The plant fiber powder is activated, and then a plasticizer and diphenylmethane diisocyanate are added for hydrophobic treatment to obtain a mixture; polybutylene succinate, a coupling agent, and an antioxidant are added to the mixture, and the mixture is blended and extruded to obtain a cellulose composite; The grafting agent is methylene succinic acid; The substrate sheet is a substrate sheet obtained by blending and extruding polyethylene terephthalate and polybutylene succinate.
2. The glitter powder according to claim 1, characterized in that: The plant fiber powder is any one of corn straw powder, wheat straw powder and rice straw powder.
3. The glitter powder according to claim 1, characterized in that: The activation treatment of the plant fiber powder is as follows: soaking the plant fiber powder in an alkaline solution and reacting it at 50-60° C. for 1-2 hours; after the reaction is completed, filtering, washing and drying to obtain the activated plant fiber powder.
4. The glitter powder according to claim 1, characterized in that: The plasticizer is 1-butyl-3-methylimidazolium chloride.
5. The glitter powder according to claim 1, characterized in that: The coupling agent is a silane coupling agent.
6. The glitter powder according to claim 1, characterized in that: The antioxidant is a hydroxylamine antioxidant.
7. The glitter powder according to claim 1, characterized in that: The pigments include iron oxide red, iron oxide black, titanium white, zinc chrome yellow, lead chrome green, zinc white, iron blue and cobalt blue.
8. The glitter powder according to claim 1, characterized in that: The preparation method of glitter powder comprises the following steps: 1) Preparation of substrate sheet 2) Cellulose complex 3) Preparation of coating slurry The cellulose composite, the grafting agent and the pigment are mixed to obtain a coating slurry; 4) Coating The substrate sheet is coated with a printed coating slurry; after drying, the sheet is cut to obtain glitter powder.
Citation Information
Patent Citations
Coir / polybutylene succinate composite material and preparation method thereof
CN105440602A