Battery finishing tape, winding core assembly and secondary battery
By using a combined adhesive of epoxy resin and polyvinyl acetate in the battery closing tape, the problem of insufficient stability in the electrolyte is solved, high stability and good bonding performance of the battery are achieved, and the battery's durability is improved. Cycle performance and production efficiency.
Patent Information
- Application Number
- CN202410982165.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-22
AI Technical Summary
The existing battery closing tape has insufficient stability in the electrolyte and is prone to side reactions with the electrolyte, resulting in a decrease in bonding performance and easily leading to loss of battery capacity and peeling off of the closing tape.
A combination of epoxy resin and polyvinyl acetate is used as the adhesive for the adhesive layer. By adjusting their mass ratio and adding fillers, plasticizers and organic solvents, the adhesion and compatibility are improved to form a high-viscosity finishing tape. , to maintain stability and adhesion in the electrolyte.
It achieves high stability and good bonding performance in the electrolyte, reduces the loss of battery capacity and the occurrence of tape peeling off, and improves the cycle performance and production efficiency of the battery.
Smart Images

Figure SMS_18 
Figure SMS_19 
Figure QLYQS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of batteries, and in particular to a battery finishing tape, a winding core assembly and a secondary battery. Background Art
[0002] At present, with the rapid popularization of new energy vehicles and the continuous expansion of the scale of the power battery industry, the demand for lithium batteries has increased significantly, and there is a huge demand for the tailing tape used in the secondary battery industry. In the preparation process of secondary batteries, one of the processes is to stack the positive electrode sheet, the diaphragm and the negative electrode sheet in order, so that the diaphragm is in the middle of the positive and negative electrodes to play an isolation role, and then the stacked electrode sheet and the diaphragm are wound to obtain a roll core. The outer surface of the battery roll core is provided with a diaphragm tail end and a tailing tape. The tailing tape includes an adhesive layer and a substrate. The adhesive layer is adhered to the diaphragm tail end along the extension direction of the diaphragm tail end, and the substrate is adhered to one side of the adhesive layer, thereby ensuring that the battery roll core will not fall apart. The roll core is then placed in the aluminum-plastic film bag that has been punched and formed, and the electrolyte is injected.
[0003] The solvent of traditional electrolyte is mainly carbonate compounds, which contain more polar functional groups such as carbonyl and carboxyl. The end tape used in existing battery rolls is not stable enough in the electrolyte. The high molecular polymer epoxy resin with strong adhesion in the end tape contains more epoxy groups. These epoxy groups will react with carbonyl and carboxyl groups in the electrolyte, causing chemical changes in the epoxy resin and losing its original properties. Especially under high temperature conditions, when there are more side reactions between the glue and the electrolyte, the active lithium in the electrolyte will be continuously consumed, resulting in battery capacity loss.
[0004] The closing tape used in existing battery rolls is prone to side reactions with the electrolyte. During the long-term charge and discharge cycle of lithium-ion batteries, the closing tape is prone to aging and the bonding performance is reduced. In particular, during the charge and discharge process of the battery, the electrode will continue to shrink and expand, which can easily cause the closing tape to fall off. Therefore, how to overcome the above-mentioned technical problems and defects has become a key issue that needs to be resolved. Summary of the invention
[0005] In view of the problems that the existing finishing tape is prone to side reactions with the electrolyte and the stability of the finishing tape in the electrolyte is insufficient, the present invention provides a battery finishing tape, a core assembly and a secondary battery.
[0006] The technical solution adopted by the present invention to solve the above technical problems is as follows:
[0007] On one hand, the present invention provides a battery finishing tape, including an adhesive layer and a substrate, wherein the adhesive layer is covered on one side of the substrate, and the adhesive layer is obtained by curing the adhesive layer glue, wherein the adhesive layer glue includes an adhesive, and the adhesive includes epoxy resin and polyvinyl acetate.
[0008] Optionally, the weight average molecular weight of the epoxy resin is 100,000-300,000.
[0009] Optionally, based on the total weight of the adhesive being 100%, the mass percentage of the epoxy resin in the adhesive is 50%-70%; the mass percentage of the polyvinyl acetate in the adhesive is 30%-50%.
[0010] Optionally, the bonding layer glue also includes a filler, a plasticizer and a first organic solvent, the plasticizer includes one or more of dioctyl phthalate, dihexyl adipate, triethylene glycol diisooctanoate, benzimidazolone yellow, diol isomeric fatty acid complex ester, dioctyl sebacate or dibutyl sebacate; the filler includes one or more of calcium carbonate, silicon micropowder, mica powder, aluminum hydroxide; the first organic solvent includes one or more of toluene, butanone, and ethyl acetate.
[0011] Optionally, based on the total weight of the adhesive layer as 100%, the mass percentage of the adhesive in the adhesive layer glue is 60%-80%; the mass percentage of the filler in the adhesive layer glue is 5%-25%; the mass percentage of the plasticizer in the adhesive layer glue is 5%-25%; and the mass percentage of the first organic solvent in the adhesive layer glue is 5%-20%.
[0012] Optionally, the substrate includes one or more of a PP base film, a PE base film, a BOPP base film or a PET base film.
[0013] On the other hand, the present invention provides a winding core assembly, comprising a positive electrode sheet, a negative electrode sheet, a separator and the battery finishing tape as described above, wherein the positive electrode sheet, the separator and the negative electrode sheet are stacked and wound to form a winding core, and a separator finishing end is provided on the outer surface of the winding core, and the separator finishing end is fixed by the battery finishing tape.
[0014] Another aspect of the present invention provides a secondary battery, comprising the core assembly as described above, an electrolyte and a shell, wherein the core assembly is placed in the shell, and the electrolyte comprises a lithium salt, a second organic solvent and a boron trifluoride additive.
[0015] Optionally, the boron trifluoride additive includes one or more of the following compounds:
[0016] , , , , .
[0017] Optionally, based on the total weight of the electrolyte being 100%, the mass percentage of the lithium salt in the electrolyte is 10%-18%; the mass percentage of the second organic solvent in the electrolyte is 80%-85%; the mass percentage of the boron trifluoride additive in the electrolyte is W%, and W satisfies: 0.5≤W≤3;
[0018] Taking the total weight of the adhesive layer glue as 100%, the mass percentage of the epoxy resin in the adhesive layer glue is A%, and A satisfies: 50≤A≤70;
[0019] The A and W satisfy the relationship: 0.714≤(W 100) / A≤6.
[0020] According to the battery finishing tape provided by the present invention, the present invention selects high-molecular polymer epoxy resin and polyvinyl acetate with strong adhesion as the main resin in the adhesive formula of the adhesive layer. The adhesive layer can swell quickly in the carbonate electrolyte and will not block the normal migration of lithium ions; moreover, the adhesive layer compounded by epoxy resin and polyvinyl acetate has good tolerance in the electrolyte, and can avoid the corrosion of the adhesive layer by the electrolyte during long-term circulation. At the same time, the adhesive layer has high electrochemical stability, which can avoid electrochemical reactions under the action of voltage, and thus can maintain a high adhesion during the long-term circulation of the battery, and avoid the battery finishing tape from falling off. DETAILED DESCRIPTION
[0021] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention clearer, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0022] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods; the materials and reagents used are reagents and materials that can be obtained from commercial channels unless otherwise specified.
[0023] In one embodiment, the present invention provides a battery finishing tape, including an adhesive layer and a substrate, wherein the adhesive layer is covered on one side of the substrate, and the adhesive layer is obtained by curing the adhesive layer glue, and the adhesive layer glue includes an adhesive, and the adhesive includes epoxy resin and polyvinyl acetate.
[0024] In the production process of soft-pack polymer batteries, the winding end of the battery core needs to be fixed. The existing battery core winding end structure usually adopts a winding structure for the end fixing, and the middle position of the battery core is wound and fixed with adhesive tape to ensure that the battery core will not spread out.
[0025] The adhesive layer of the present invention uses epoxy resin and polyvinyl acetate, both of which have strong adhesive properties, as main resins. The adhesive layer has good bonding effect and can swell quickly in carbonate electrolyte.
[0026] At present, the electrolyte solvents used in lithium-ion batteries mainly include carbonate solvents such as dimethyl carbonate, ethylene carbonate, and ethyl methyl carbonate. The chemical structure of carbonate contains a large number of polar functional groups such as carbonyl and carboxyl. Epoxy resin contains a large number of epoxy groups. When only epoxy resin is used as the main resin of adhesives in battery finishing tape, these epoxy groups will react with carbonyl and carboxyl groups in the electrolyte, causing chemical changes in the epoxy resin and losing its original properties. Under high temperature conditions, the side reactions between the adhesive and the electrolyte are intensified, generating more acidic byproducts. The acidic byproducts will decompose lithium salts, causing active lithium in the battery electrolyte and resulting in battery capacity loss.
[0027] The adhesive of the battery finishing tape of the present application includes epoxy resin and polyvinyl acetate at the same time; polyvinyl acetate is not easy to react violently with the carbonyl and carboxyl groups in the electrolyte, so its compatibility with the electrolyte is good, but its adhesion is worse than that of epoxy resin. Polyvinyl acetate is easily soluble in carbonate solvents, which can significantly increase the swelling rate of the adhesive layer in the electrolyte, making the prepared adhesive layer more susceptible to corrosion by lithium hexafluorophosphate in the electrolyte, thereby achieving the effect of rapid swelling, and realizing the rapid swelling of the adhesive layer in the electrolyte without blocking the normal migration of lithium ions. Epoxy resin ensures the adhesion ratio of the adhesive layer glue, so the combination of epoxy resin and polyvinyl acetate can take into account the adhesion of the battery finishing tape and its compatibility with the electrolyte.
[0028] In some embodiments, epoxy resin has good adhesion. The higher the proportion of epoxy resin in the adhesive layer glue, the better the adhesion of the finishing tape, which can prevent the finishing tape from falling off due to the shrinkage and expansion of the pole piece during the battery charging and discharging process. Using high-viscosity finishing tape can greatly reduce the abnormal rate of core unravelling caused by the weak adhesion of the tape during the core production process, which is beneficial to improving the production efficiency of the core factory; and using high-viscosity finishing tape can reduce the hard expansion thickness of the core at the end during the battery cycle.
[0029] In one embodiment, the weight average molecular weight of the epoxy resin is 100,000-300,000.
[0030] If the molecular weight of the epoxy resin is too high, the side reaction with the electrolyte will be aggravated and the capacity retention rate will be significantly reduced. If the molecular weight is too low, the adhesion of the tape will be reduced. During the core production process, the abnormal rate of core unravelling caused by the weak adhesion of the tape will be greatly increased, reducing the production efficiency of the core factory.
[0031] In some embodiments, the molecular weight of the polyvinyl acetate is 2-5w. If the molecular weight is too high, the adhesive layer of the battery separator tape will swell slowly in the electrolyte. If the molecular weight is too low, the water absorption rate of the battery separator tape will be high, which will affect the electrolyte performance.
[0032] In one embodiment, based on the total weight of the adhesive being 100%, the mass percentage of the epoxy resin in the adhesive is 50%-70%; the mass percentage of the polyvinyl acetate in the adhesive is 30%-50%.
[0033] In a preferred embodiment, the mass percentage of the epoxy resin in the adhesive is 55%-65%. Specifically, the mass percentage of the epoxy resin in the adhesive is 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69% or 70%, any one of the values or a range consisting of any two values.
[0034] In a preferred embodiment, the mass percentage of polyvinyl acetate in the adhesive is 35%-45%. Specifically, the mass percentage of polyvinyl acetate in the adhesive is 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49% or 50%, any one of the values or a range consisting of any two values.
[0035] Moreover, the adhesive made with polyvinyl acetate has better anti-aging and weather resistance.
[0036] In one embodiment, the bonding layer glue also includes a filler, a plasticizer and a first organic solvent, the plasticizer includes one or more of dioctyl phthalate, dihexyl adipate, triethylene glycol diisooctanoate, benzimidazolone yellow, diol isomeric fatty acid complex ester, dioctyl sebacate or dibutyl sebacate; the filler includes one or more of calcium carbonate, silicon micropowder, mica powder, aluminum hydroxide; the first organic solvent includes one or more of toluene, butanone, and ethyl acetate.
[0037] Specifically, during the relevant experiments of the present invention, it was found that when the above plasticizers were used, the adhesive properties of the prepared adhesive layer were better.
[0038] In one embodiment, the calcium carbonate included in the filler is nano-calcium carbonate, and the silicon micropowder is silicone-modified silicon micropowder; the adhesive layer provided by this solution uses nano-calcium carbonate and / or silicone-modified silicon micropowder as inorganic filler, and the silicon micropowder modified by nano-calcium carbonate and / or silicone can be better dispersed and filled in the main resin of the adhesive, and can reduce the shrinkage of the resin during the curing process of the adhesive, and can also increase the adhesion between the adhesive layer formed by the adhesive and the interface of the adhered object.
[0039] In one embodiment, taking the total weight of the adhesive layer glue as 100%, the mass percentage of the adhesive in the adhesive layer glue is 60%-80%; the mass percentage of the filler in the adhesive layer glue is 5%-25%; the mass percentage of the plasticizer in the adhesive layer glue is 5%-25%; and the mass percentage of the first organic solvent in the adhesive layer glue is 5%-20%.
[0040] In a preferred embodiment, the mass percentage of the adhesive in the adhesive layer is 65%-75%. Specifically, the mass percentage of the adhesive in the adhesive layer is 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79% or 80%, any one of the values or a range consisting of any two values.
[0041] In a preferred embodiment, the mass percentage of the filler in the adhesive layer is 10%-20%. Specifically, the mass percentage of the filler in the adhesive layer is 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24% or 25%, any one of the values or a range consisting of any two of the values.
[0042] In a preferred embodiment, the mass percentage of the plasticizer in the adhesive layer is 10%-20%. Specifically, the mass percentage of the plasticizer in the adhesive layer is 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24% or 25%, any one of the values or a range consisting of any two values.
[0043] In a preferred embodiment, the mass percentage of the first organic solvent in the adhesive layer is 10%-15%. Specifically, the mass percentage of the first organic solvent in the adhesive layer is any point value among 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% or 20%, or a range value consisting of any two point values.
[0044] Specifically, when the content of the adhesive is within the above range, it has a good bonding effect, but is not easy to have side reactions with the electrolyte; when the content of the filler is within the above range, it can improve the adhesion and heat resistance, if the filler is too much, it will affect the fluidity of the glue; when the content of the plasticizer is within the above range, it has the effect of weakening the secondary bonds between resin molecules, increasing the mobility of the resin molecular bonds, reducing the crystallinity of the resin molecules, increasing the plasticity of the resin molecules, making them more flexible and easy to process, if the plasticizer is too much, it will affect the bonding effect; when the content of the first organic solvent is within the above range, the adhesive solvent has a good dissolving material, which can effectively help the solvent-based adhesive to dissolve, too much will affect the bonding effect, and too little will have a poor dissolving effect on the adhesive.
[0045] In one embodiment, the substrate includes one or more of a PP base film, a PE base film, a BOPP base film or a PET base film.
[0046] In a preferred embodiment, the thickness of the substrate is 6-10 μm.
[0047] Preferably, the adhesive layer is directly compounded with the substrate, and the adhesive layer is made of an adhesive, and the adhesive includes epoxy resin and polyvinyl acetate; the substrate and the adhesive layer are tightly bonded and not easy to peel off. The substrate can provide good strength and flexibility for the adhesive layer, and the adhesive layer made of epoxy resin and polyvinyl acetate as adhesives has better adhesion, can maintain good adhesion with the adhered object, and can also be tightly adhered to the substrate made of polyethylene.
[0048] On the other hand, the present invention provides a winding core assembly, comprising a positive electrode sheet, a negative electrode sheet, a separator and the battery finishing tape as described above, wherein the positive electrode sheet, the separator and the negative electrode sheet are stacked and wound to form a winding core, and a separator finishing end is provided on the outer surface of the winding core, and the separator finishing end is fixed by the battery finishing tape.
[0049] In some embodiments, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer coated on one side or both sides of the positive electrode current collector, and the positive electrode active material layer includes a positive electrode active material, a positive electrode conductor and a positive electrode binder.
[0050] In some embodiments, the positive electrode active material is selected from one or more of lithium iron phosphate (LFP), lithium iron manganese phosphate (LMFP), lithium cobalt oxide (LCO), lithium nickel cobalt manganese oxide (NCM), and lithium manganese oxide (LMO);
[0051] In some embodiments, the positive electrode conductive agent includes one or more of graphite, superconducting carbon, acetylene black, carbon black, carbon nanotubes, graphene, carbon nanofibers, metal powder, metal fibers, and polyphenylene derivatives;
[0052] In some embodiments, the positive electrode binder includes one or more of polyvinylidene fluoride, polytetrafluoroethylene, vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylic resin.
[0053] In some embodiments, the mass percentage of each component in the positive electrode active material layer is: 96-98wt% of positive electrode active material, 0.5-2wt% of positive electrode conductive agent, and 1.0-2.0wt% of positive electrode binder.
[0054] When the mass ratio of the positive electrode active material in the positive electrode active material layer is within the above range, the positive electrode sheet can have a higher lithium removal and lithium insertion capacity, and the lithium-ion battery can have a higher capacity.
[0055] The positive electrode current collector is selected from a metal material that can conduct electrons. Preferably, the positive electrode current collector includes one or more of copper, nickel, tin, copper, and stainless steel. In a more preferred embodiment, the positive electrode current collector is selected from aluminum foil.
[0056] The positive electrode sheet can be prepared according to conventional methods in the art. For example, the positive electrode active material layer is usually prepared by coating a positive electrode slurry made of a positive electrode active material, a positive electrode conductive agent, a positive electrode binder and any other components on a positive electrode current collector, followed by drying and cold pressing. The solvent can be N-methylpyrrolidone (NMP), but is not limited thereto.
[0057] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer coated on one or both sides of the negative electrode current collector, and the negative electrode active material layer includes a negative electrode active material, a negative electrode conductor, a negative electrode binder and a negative electrode thickener.
[0058] In some embodiments, the negative electrode active material is selected from one or more of artificial graphite, natural graphite, silicon-oxygen material, silicon-carbon material, hard carbon, soft carbon, and mesophase carbon microspheres;
[0059] In some embodiments, the negative electrode conductive agent includes one or more of graphite, superconducting carbon, acetylene black, carbon black, carbon nanotubes, graphene, carbon nanofibers, metal powder, metal fibers, and polyphenylene derivatives;
[0060] In some embodiments, the negative electrode binder includes one or more of styrene-butadiene rubber, polyacrylic acid, sodium polyacrylate, polyacrylamide, polyvinyl alcohol, and polymethacrylic acid.
[0061] In some embodiments, the negative electrode thickener includes one or more of sodium alginate, sodium carboxymethyl cellulose, and carboxymethyl chitosan.
[0062] In some embodiments, the mass percentage of each component in the negative electrode active material layer is: 96%-97% of negative electrode active material, 0.5%-1.5% of negative electrode conductor, 1%-2% of negative electrode binder and 0.5%-1.5% of negative electrode thickener.
[0063] When the mass ratio of the negative electrode active material in the negative electrode active material layer is within the above range, lithium ions can reach the negative electrode active material interface faster, and the improvement effects of kinetics, cycle, etc. are better.
[0064] The negative electrode current collector is selected from metal materials that can conduct electrons. Preferably, the negative electrode current collector includes one or more of Al, Ni, tin, copper, and stainless steel. In a more preferred embodiment, the negative electrode current collector is selected from copper foil.
[0065] The negative electrode sheet can be prepared according to conventional methods in the art. For example, the negative electrode active material layer is usually prepared by coating a negative electrode slurry made of a negative electrode active material, a negative electrode conductive agent, a negative electrode binder, a negative electrode thickener and any other components on a negative electrode current collector, followed by drying and cold pressing. The solvent can be an aqueous solvent, but is not limited thereto.
[0066] Specifically, it also includes a diaphragm, which can be various diaphragm materials suitable for lithium-ion batteries or sodium-ion batteries in the art, for example, it can be a combination of one or more including but not limited to single-layer PP (polypropylene), single-layer PE (polyethylene), double-layer PP / PE, double-layer PP / PP, three-layer PP / PE / PP, polyvinylidene fluoride, aramid, polyethylene terephthalate, polytetrafluoroethylene, polyacrylonitrile, polyimide, polyamide, polyester and natural fiber.
[0067] The battery finishing tape of the present invention adopts epoxy resin and polyvinyl acetate as adhesives. Epoxy resin is a high molecular polymer with strong adhesion. Epoxy resin as an adhesive can improve the adhesion of the tape. During the production of the core assembly, the abnormal rate of core unwinding caused by the weak adhesion of the battery finishing tape will be greatly reduced, which is beneficial to improving the production efficiency of the core assembly. Moreover, the use of high-viscosity finishing tape can reduce the hard expansion thickness of the core at the end during the battery cycle. The adhesive of the battery finishing tape of the present application includes epoxy resin and polyvinyl acetate at the same time. Polyvinyl acetate is not easy to react violently with the carbonyl and carboxyl groups in the electrolyte, so it has good compatibility with the electrolyte, but its adhesion is worse than that of epoxy resin. Polyvinyl acetate is easily soluble in carbonate solvents, which can significantly increase the swelling rate of the adhesive layer in the electrolyte, making the adhesive layer more susceptible to corrosion by lithium hexafluorophosphate in the electrolyte, thereby achieving a rapid swelling effect, and realizing rapid swelling of the adhesive layer in the electrolyte without blocking the normal migration of lithium ions. Epoxy resin ensures the adhesion of the adhesive layer, so the combination of epoxy resin and polyvinyl acetate can take into account the adhesion of the battery finishing tape and its compatibility with the electrolyte.
[0068] Another aspect of the present invention provides a secondary battery, comprising the core assembly as described above, an electrolyte and a shell, wherein the core assembly is placed in the shell, and the electrolyte comprises a lithium salt, a second organic solvent and a boron trifluoride additive.
[0069] The higher the amount of high-viscosity epoxy resin used, the better the adhesion of the tape. The abnormal rate of core unravelling caused by poor adhesion of the tape during the core production process will be greatly reduced, which is beneficial to improving the production efficiency of the core factory; and the use of high-viscosity finishing tape can reduce the hard expansion thickness of the core at the end during the battery cycle; however, when the amount of high-viscosity epoxy resin used is high, its side reaction with the electrolyte will intensify, and the battery capacity retention rate will be significantly reduced; by adding boron trifluoride additives to the electrolyte, a stable interface protective film can be formed at the positive and negative electrode interfaces at the same time, effectively improving the cycle performance of the core. At the same time, such additives can also inhibit the side reactions of epoxy resin and electrolyte.
[0070] In some embodiments, the lithium salt as the electrolyte salt can be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate and lithium tetrafluorooxalatophosphate.
[0071] In some embodiments, the second organic solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane sulfone, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.
[0072] In some embodiments, the electrolyte may also optionally include film-forming additives, such as negative electrode film-forming additives, positive electrode film-forming additives, and may also include other additives that can improve certain properties of the battery, such as additives that improve the overcharge performance of the battery, additives that improve the high or low temperature performance of the battery, etc.
[0073] Production of secondary batteries:
[0074] The positive electrode sheet, the separator and the negative electrode sheet are stacked in order, so that the separator is in the middle of the positive and negative electrodes to play a role of isolation, and then the stacked electrode sheets and the separator are wound to obtain a winding core. The outer surface of the battery winding core is provided with a separator tail end and a tail tape, and the tail tape includes an adhesive layer and a substrate. The adhesive layer is adhered to the separator tail end along the extension direction of the separator tail end, and the substrate is adhered to one side of the adhesive layer to obtain a winding core assembly.
[0075] The core assembly is placed in an aluminum-plastic film bag formed by punching and forming, and the non-aqueous electrolyte prepared above is injected into the baked and dried core. After vacuum packaging, standing, forming and other processes, a lithium-ion battery is obtained.
[0076] In one embodiment, the boron trifluoride additive includes one or more of the following compounds:
[0077] , , , , .
[0078] Specifically, compound I is boron trifluoride·pyridine, compound II is boron trifluoride·triphenylphosphine oxide, compound III is boron trifluoride·pyrazine, compound IV is boron trifluoride·triazine, and compound V is boron trifluoride·trimethyl phosphate.
[0079] When the usage of high-viscosity epoxy resin is high, its side reaction with the electrolyte will intensify and the battery capacity retention rate will be significantly reduced. By adding boron trifluoride additives to the electrolyte, a stable interface protection film can be formed at the interface of the positive and negative electrodes at the same time, effectively improving the cycle performance of the core assembly. At the same time, such additives can also inhibit the side reactions of epoxy resin and electrolyte.
[0080] By adding boron trifluoride additives to the electrolyte, the compatibility of the battery finishing tape and the electrolyte can be improved. While enhancing the peel strength of the finishing tape, the side reaction between the electrolyte and the adhesive layer of the finishing tape can be reduced, thereby improving the high-temperature cycle performance and thickness expansion rate of the battery.
[0081] In one embodiment, the total weight of the electrolyte is 100%, the mass percentage of the lithium salt in the electrolyte is 10%-18%; the mass percentage of the second organic solvent in the electrolyte is 80%-85%; the mass percentage of the boron trifluoride additive in the electrolyte is W%, and W satisfies: 0.5≤W≤3;
[0082] Taking the total weight of the adhesive layer glue as 100%, the mass percentage of the epoxy resin in the adhesive layer glue is A%, and A satisfies: 50≤A≤70;
[0083] The A and W satisfy the relationship: 0.714≤(W 100) / A≤6.
[0084] Specifically, the mass percentage of the lithium salt in the electrolyte is any one of 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17% or 18%, or a range consisting of any two of the values. In a preferred embodiment, the mass percentage of the lithium salt in the electrolyte is 12%-16%.
[0085] Specifically, the mass percentage of the second organic solvent in the electrolyte is any one of 80%, 81%, 82%, 83%, 84% or 85%, or a range consisting of any two of the values. In a preferred embodiment, the mass percentage of the second organic solvent in the electrolyte is 81%-84%.
[0086] Specifically, the mass percentage of the boron trifluoride additive in the electrolyte is 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9% or 3.0%, or any range of any two points. In a preferred embodiment, the mass percentage of the boron trifluoride additive in the electrolyte is 1%-2%. In one embodiment, A and W satisfy the relationship: 0.714≤(W 100) / A≤6.
[0087] Specifically, A and W satisfy the relationship: (W The ratio of 100) / A is any value among 0.714, 0.8, 1, 1.2, 1.4, 1.6, 1.8, 2.0, 2.2, 2.4, 2.6, 2.8, 3.0, 3.2, 3.4, 3.6, 3.8, 4.0, 8.2, 4.4, 4.6, 4.8, 5.0, 5.2, 5.4, 5.6, 5.8 or 6.0, or a range consisting of any two values.
[0088] (W When (W 100) / A is greater than 6, the side reaction between epoxy resin and electrolyte is aggravated and the capacity retention rate is significantly reduced; When 100) / A is less than 0.714, the adhesion of the finishing tape is reduced. During the core production process, the abnormal rate of core unravelling caused by the weak adhesion of the finishing tape will be greatly increased, reducing the production efficiency of the core assembly.
[0089] In a preferred embodiment, A and W satisfy the relationship: 1≤(W 100) / A≤5.
[0090] The secondary battery disclosed in the embodiment of the present application can be applied to an electrical device that uses a battery as a power source, or to various energy storage systems that use a battery as an energy storage element. The electrical device may be, but is not limited to, a mobile phone, a tablet, a laptop computer, an electric toy, an electric tool, a battery car, an electric car, a ship, a spacecraft, and the like. An electric car may be a fuel car, a gas car, or a new energy car, and a new energy car may be a pure electric car, a hybrid car, or an extended-range car, etc.; a spacecraft includes an airplane, a rocket, a space shuttle, and a spacecraft, etc.; an electric toy includes a fixed or mobile electric toy, such as a game console, an electric car toy, an electric ship toy, and an electric airplane toy, etc.; an electric tool includes a metal cutting electric tool, a grinding electric tool, an assembly electric tool, and an electric tool for railways, such as an electric drill, an electric grinder, an electric wrench, an electric screwdriver, an electric hammer, an impact drill, a concrete vibrator, and an electric planer, etc.
[0091] The present invention is further described below by way of examples.
[0092] Table 1 Design of battery finishing tape and electrolyte added in Examples 1-9 and Comparative Examples 1-7;
[0093]
[0094] Example 1
[0095] This embodiment is used to illustrate the battery finishing tape, the core assembly and the secondary battery disclosed in the present invention; and includes the following operating steps:
[0096] Preparation of battery finishing tape: polyvinyl acetate: dioctyl phthalate: calcium carbonate: toluene are mixed evenly in a mass ratio of 5:1:1:5, and epoxy resin accounting for 50% of the total adhesive mass is added to the adhesive to obtain a bonding layer glue. The bonding layer glue is evenly coated on the substrate and cured to obtain an adhesive layer, and the substrate is polyimide.
[0097] Preparation of non-aqueous electrolyte: EC (ethylene carbonate), PC (propylene carbonate), and PP (propyl propionate) were mixed at a mass ratio of 1:1:1 as the second organic solvent. 0.5% boron trifluoride·pyridine was added to the second organic solvent, and after mixing evenly, LiPF6 was added to obtain a non-aqueous electrolyte with a LiPF6 concentration of 1.1 mol / L.
[0098] Preparation of positive electrode sheet: The positive electrode active material lithium nickel cobalt manganese oxide (LiNi 0.8 Co 0.1 Mn 0.1 O2), positive electrode conductive agent CNT (Carbon Nanotube, carbon nanotube), positive electrode binder PVDF (polyvinylidene fluoride), mixed at a mass ratio of 95:1.5:1.5. Stir and mix thoroughly in N-methylpyrrolidone solvent to form a uniform positive electrode slurry. Apply the positive electrode slurry on the positive electrode current collector aluminum foil, dry, and cold press to obtain a positive electrode sheet.
[0099] Preparation of negative electrode sheet: Graphite as negative electrode active material, acetylene black as negative electrode conductive agent, styrene butadiene rubber as negative electrode binder, and sodium carboxymethyl cellulose as negative electrode thickener are fully stirred and mixed in deionized water solvent at a mass ratio of 96:1.2:1.5:1.3 to form a uniform negative electrode slurry. The negative electrode slurry is coated on the negative electrode current collector copper foil, dried, and cold pressed to obtain a negative electrode sheet.
[0100] Production of diaphragm: PE porous polymer film is used as diaphragm.
[0101] Production of secondary batteries:
[0102] The positive electrode sheet, the separator and the negative electrode sheet are stacked in order, so that the separator is in the middle of the positive and negative electrodes to play a role of isolation, and then the stacked electrode sheets and the separator are wound to obtain a winding core. The outer surface of the battery winding core is provided with a separator tail end and a tail tape, and the tail tape includes an adhesive layer and a substrate. The adhesive layer is adhered to the separator tail end along the extension direction of the separator tail end, and the substrate is adhered to one side of the adhesive layer to obtain a winding core assembly.
[0103] The core assembly is placed in an aluminum-plastic film bag formed by punching and forming, and the non-aqueous electrolyte prepared above is injected into the baked and dried core. After vacuum packaging, standing, forming and other processes, a lithium-ion battery is obtained.
[0104] Embodiments 2 to 9
[0105] Examples 2 to 9 are used to illustrate the battery finishing tape, the core assembly and the secondary battery disclosed in the present invention, and include most of the operation steps in Example 1, except that:
[0106] The components and contents of the electrolyte additives and the components and contents of the adhesives shown in Table 1 were used.
[0107] Comparative Examples 1 to 7
[0108] Comparative Examples 1 to 7 are used to illustrate the battery finishing tape, the core assembly and the secondary battery disclosed in the present invention, and include most of the operation steps in Example 1, except that:
[0109] Performance Testing
[0110] The lithium ion batteries prepared in Examples 1 to 9 and Comparative Examples 1 to 7 were subjected to the following performance tests:
[0111] 45℃ Cycle Test
[0112] The test method is: charge the lithium-ion battery to 4.45V at 1C constant current and constant voltage in a 45±2℃ constant temperature box, cut off the current at 0.05C, and then discharge it to 3V at 1C. Perform multiple charge and discharge cycles under the above conditions. Calculate the capacity retention rate of the battery after 800 cycles, with 5 batteries in each group.
[0113] Capacity retention rate (%) = discharge capacity of the 800th cycle (mAh) / discharge capacity of the third cycle (mAh) × 100%
[0114] Thickness expansion rate (%) = (thickness of the 800th cycle - thickness of the third cycle / ) thickness of the third cycle × 100%
[0115] Peel strength test of the adhesive tape after soaking in electrolyte:
[0116] The adhesive tape was immersed in the electrolyte prepared in Comparative Examples 1-4 and Examples 1-11 at 85°C for 4 hours, and then hot-pressed at 85°C and 1 MPa, and the peel strength of the finishing adhesive tape was tested;
[0117] The test results are shown in Table 2
[0118] Table 2 Test results of Examples 1-9 and Comparative Examples 1-7
[0119]
[0120] The data of Comparative Examples 1-2 and Examples 1-3 show that when boron trifluoride additives are added, the cycle capacity retention rate and cycle thickness expansion of the core are improved, and the peel strength of the end-tape is also enhanced. This is due to the fact that the nitrogen-containing heterocyclic rings and phosphate groups in the boron trifluoride additives can participate in film formation on the positive and negative electrode surfaces, and the boron trifluoride groups can neutralize the acidic substances produced by the side reaction of the epoxy resin in the end-tape with the carbonate solvent of the electrolyte, thereby improving the compatibility of the end-tape with the electrolyte.
[0121] The data of Comparative Examples 2-3 and Example 1 show that when the content of boron trifluoride additives is too low, the significant effect of protecting the battery electrode interface and inhibiting the side reaction between the finishing tape and the electrolyte cannot be achieved, and the peel strength of the finishing tape is low. When the content of boron trifluoride additives is too high, the increase in interface impedance is not conducive to the improvement of cycle performance.
[0122] The data of Comparative Examples 4-5 and Comparative Example 2 show that other boron-containing additives cannot achieve the effect of the boron trifluoride additives in the present invention.
[0123] The data of Comparative Examples 2 and 6-7 and Examples 4-5 show that when the epoxy resin content is too low, the adhesion of the tailing tape is low, and the tail of the core is easy to spread during the charge and discharge process, causing the core thickness to increase. When the epoxy resin content is too high, the side reaction with the electrolyte increases sharply, and the cycle capacity retention rate decreases. As the epoxy resin content increases, the peel strength of the tailing tape increases, the cycle thickness expansion rate improves, and the cycle capacity deteriorates.
[0124] The data of Examples 6 to 9 and Example 1 show that when the boron trifluoride additive is other substances in the claims of the present invention, the improvement effect is consistent.
[0125] The data of Comparative Examples 2, 3, 6, 7 and Examples 1 to 5 show that only when 0.5≤W≤3, 50≤A≤70, and 0.714≤(W The comprehensive performance of the battery is best when 100) / A≤6.
[0126] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A secondary battery, characterized in that: It includes a core assembly, an electrolyte and a shell, wherein the core assembly is placed in the shell, and the electrolyte includes a lithium salt, a second organic solvent and a boron trifluoride additive; Taking the total weight of the electrolyte as 100%, the mass percentage of the lithium salt in the electrolyte is 10%-18%; the mass percentage of the second organic solvent in the electrolyte is 80%-85%; the mass percentage of the boron trifluoride additive in the electrolyte is W%, and W satisfies: 0.5≤W≤3; The boron trifluoride additive includes one or more of the following compounds: 、 、 、 、 ; The winding core assembly comprises a positive electrode sheet, a negative electrode sheet, a separator and a battery tailing tape. The positive electrode sheet, the separator and the negative electrode sheet are stacked and wound to form a winding core. The outer surface of the winding core is provided with a separator tailing end, and the separator tailing end is fixed by the battery tailing tape. The battery finishing tape comprises an adhesive layer and a substrate, wherein the adhesive layer is covered on one side of the substrate, and the adhesive layer is obtained by curing the adhesive layer glue, wherein the adhesive layer glue comprises an adhesive, and the adhesive comprises epoxy resin and polyvinyl acetate; Taking the total weight of the adhesive layer glue as 100%, the mass percentage of the epoxy resin in the adhesive layer glue is A%, and A satisfies: 50≤A≤70; A and W satisfy the relationship: 0.714≤(W*100) / A≤6.
2. The secondary battery according to claim 1, characterized in that: The weight average molecular weight of the epoxy resin is 100,000-300,000.
3. The secondary battery according to claim 1, characterized in that: Taking the total weight of the adhesive as 100%, the mass percentage of the epoxy resin in the adhesive is 50%-70%; the mass percentage of the polyvinyl acetate in the adhesive is 30%-50%.
4. The secondary battery according to claim 1, characterized in that: The bonding layer glue also includes a filler, a plasticizer and a first organic solvent, the plasticizer includes one or more of dioctyl phthalate, dihexyl adipate, triethylene glycol diisooctanoate, dioctyl sebacate or dibutyl sebacate; the filler includes one or more of calcium carbonate, silicon micropowder, mica powder, aluminum hydroxide; the first organic solvent includes one or more of toluene, butanone, and ethyl acetate.
5. The secondary battery according to claim 4, characterized in that: Taking the total weight of the adhesive layer glue as 100%, the mass percentage of the adhesive in the adhesive layer glue is 60%-80%; the mass percentage of the filler in the adhesive layer glue is 5%-25%; the mass percentage of the plasticizer in the adhesive layer glue is 5%-25%; and the mass percentage of the first organic solvent in the adhesive layer glue is 5%-20%.
6. The secondary battery according to claim 1, characterized in that: The substrate includes one or more of a PP base film, a PE base film, a BOPP base film or a PET base film.
Citation Information
Patent Citations
Secondary battery and electronic device
CN117480657A
Thermosetting adhesive composition
JP2010270285A