A preparation method and application of Y2O3 thin film with compactness and etching resistance
By using UV light cleaning and magnetron sputtering coating technology in chip etching equipment and combining vacuum annealing to prepare Y2O3 film, the corrosion problem of plasma on the equipment materials is solved, high density and etch resistance are achieved, and the Equipment life and reduce pollution.
Patent Information
- Application Number
- CN202410997168.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-07-24
AI Technical Summary
During the chip etching process, high-energy plasma corrodes the internal materials of the etching equipment, shortens the equipment life and generates impurity pollution, and the requirements for high-precision and high-efficiency etching increase the challenge of material etching resistance. .
A method including UV light cleaning, magnetron sputtering coating and vacuum annealing is used to prepare a Y2O3 film with denseness and etch resistance for protecting the internal materials of the etching equipment. The specific steps include substrate cleaning and presputtering. , vacuum annealing, etc.
The prepared Y2O3 film exhibits low etching rate in CF4/O2 plasma environment, has cubic phase structure, tightly arranged grains, and has no holes and defects, significantly extending the service life of the equipment and improving performance.
Smart Images

Figure CN118516652B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of etching-resistant coatings, and in particular relates to a preparation method of a Y2O3 film with compactness and etching resistance and application thereof. Background Art
[0002] Chips contain integrated circuits (ICs), which are important carriers of electronic devices. From mobile phones to computers, from cars to airplanes, chips are indispensable. More than 70% of chip manufacturing processes require the use of plasma. On the one hand, plasma can deposit thin films, and on the other hand, it can also etch. But at the same time, high-energy plasma will bombard other components and even cavities in IC equipment, causing pollution or even chip short circuits.
[0003] The etching process is to selectively remove unnecessary materials from the surface of the silicon wafer. In the process flow of modern chip manufacturing, dry etching is generally used, that is, plasma is directly used to bombard the silicon wafer to achieve the purpose of etching. It has the advantages of high controllability, good flexibility, and easy automation. However, in the etching process, highly corrosive gases and high-energy plasma are required. While the plasma etches the silicon wafer through chemical and physical effects, it will also cause serious corrosion to the inside of the etcher chamber, shortening the service life of the equipment and reducing the performance of the equipment. In addition, the reaction products produced during the etching process will volatilize and fall off, and impurity particles will be generated inside the etching chamber to contaminate the wafer. There are many parts inside the etcher chamber, such as AlN, SiC, Al and quartz, which are commonly used as parts inside the etcher chamber.
[0004] The increase in wafer size and the reduction in wafer process feature size require higher plasma energy, which poses higher challenges to the high precision, high efficiency, and high uniformity of wafer etching, as well as the requirements for semiconductor miniaturization, high-density integration, and high reliability, and puts forward more stringent requirements on the etching resistance of the internal materials of the etching equipment. Therefore, it is urgent to provide a means to protect the internal materials of the etching equipment. Summary of the invention
[0005] In view of this, the present invention provides a Y2O3 film with compactness and etching resistance, which can be used to etch internal materials of equipment to extend the service life of the equipment and improve the performance of the equipment.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A method for preparing a Y2O3 thin film having compactness and etching resistance comprises the following steps:
[0008] S1. Clean the substrate, blow dry it, and place it in a UV light cleaning machine for activation treatment;
[0009] S2, placing the substrate in step S1 in a magnetron sputtering coating machine, evacuating and heating at the same time, introducing argon gas after reaching the background vacuum, pre-sputtering the Y2O3 target material, opening the baffle after the pre-sputtering is completed, adjusting the chamber pressure, and formally starting sputtering, and taking out the substrate after sputtering is completed;
[0010] S3, vacuum annealing the substrate in step S2 at 800-1000°C, continuously introducing O2 during the annealing process, and naturally cooling the substrate in a vacuum environment after the annealing is completed, thereby completing the preparation of the Y2O3 thin film.
[0011] In some specific embodiments, preferably, the vacuum annealing temperature in step S3 is 900°C.
[0012] Furthermore, in step S1, the substrate material includes Si, AlN, SiC, Al, and quartz.
[0013] Furthermore, the cleaning in step S1 is performed using acetone, alcohol and deionized water in sequence for 10 to 20 minutes; and the drying is performed using nitrogen.
[0014] Furthermore, the UV light cleaning machine in step S1 emits an ultraviolet wavelength of 185 nm, and the activation time is 18 to 22 minutes.
[0015] Furthermore, the background vacuum in step S2 is 10 -4 Pa, the heating is such that the substrate temperature is 200° C. to 300° C., and the argon gas flow rate is 40 sccm to 100 sccm.
[0016] Furthermore, the sputtering powers of the pre-sputtering and the formal sputtering in step S2 are both 100-180 W; wherein the pre-sputtering time is 3-8 min, and the formal sputtering time is 300-400 min; and the gas pressure in the chamber during the formal sputtering is 0.6 Pa.
[0017] Furthermore, in the annealing process in step S3, the heating rate is 8-10°C / min, and the holding time is 2-3h.
[0018] Furthermore, the O2 flow rate in step S3 is 5-15 sccm.
[0019] Furthermore, the Y2O3 film thickness is ≥1 μm.
[0020] Application of the Y2O3 film prepared by the above method in etching equipment.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The preparation method of the present invention is simple and has strong adaptability. It can form a dense and etching-resistant Y2O3 film on different substrate materials (Si, AlN, SiC, Al, quartz); the prepared Y2O3 film has an etching resistance rate of less than 1.5nm / min in a CF4 / O2 plasma environment, and can reach a minimum of 1.35nm / min; the prepared Y2O3 film is a cubic phase, and the grains are arranged in irregular polygons, the arrangement is dense, there are no holes, oxygen vacancies and defects, and the density is good; it can be applied to etching equipment to improve the service life and performance of the equipment. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The Y2O3 thin film samples prepared on different substrate materials in Example 1 are shown in Figure 1, including (a) Si, (b) AlN, (c) SiC, (d) Al, and (e) quartz;
[0024] Figure 2 The figure is a comparison of the Si wafer in Example 1 before (a) and after (b) treatment using ozone in a UV light cleaning machine;
[0025] Figure 3 XRD diffraction patterns of Y2O3 thin films prepared on (a) Si, (b) AlN, (c) SiC, (d) Al, and (e) quartz substrates under vacuum annealing at 900℃ and O2 flow, and Y2O3 thin films prepared on Si substrate under (f) 900℃ air annealing, (g) 600℃ vacuum annealing with O2 flow, and (h) 300℃ vacuum annealing with O2 flow;
[0026] Figure 4 Surface SEM images of Y2O3 films prepared in (a) Example 1 and (b) Comparative Example 1. DETAILED DESCRIPTION
[0027] The present invention is further described in detail below in conjunction with specific embodiments so that those skilled in the art can understand the present invention more clearly.
[0028] Sources and physical and chemical parameters of key test materials:
[0029] The substrate materials P-type Si, AlN, SiC, Al, and quartz are all common commercially available materials with single-side polishing.
[0030] The target material Y2O3 comes from Zhongnuo New Materials, with a purity of 99.99%. The target material has a diameter of 60mm, a thickness of 3mm, and is bound to a 2mm copper backing plate.
[0031] Example 1
[0032] This embodiment provides a method for preparing a Y2O3 thin film having compactness and etching resistance, comprising the following steps:
[0033] S1. The P-type Si substrate was cleaned with acetone, alcohol and deionized water respectively under ultrasonic conditions with a power of 180W for 15 minutes, and then dried with nitrogen. Then, the organic matter on the surface of the dried P-type Si was activated for 20 minutes using ozone generated by a UV light cleaning machine (ultraviolet wavelength of 185nm), and the substrate surface was cleaned for the second time.
[0034] S2. Place the substrate processed in S1 into the vacuum chamber of the magnetron sputtering coating machine, close the chamber door, and evacuate the chamber under the joint action of the mechanical pump and the molecular pump; turn on the heating power supply during the evacuation process to make the substrate temperature reach 300°C, and wait until the background vacuum is reached for 10 -4 After the chamber pressure reaches 0.6 Pa, Ar is introduced with a flow rate of 80 sccm; the RF power supply is turned on, the power is adjusted to 140 W, and the target material is pre-sputtered for 5 minutes; after the pre-sputtering is completed, the baffle is opened, the chamber pressure is adjusted to 0.6 Pa, and formal sputtering is carried out. After sputtering for 400 minutes, the substrate is taken out and the machine is turned off.
[0035] S3. Place the substrate processed in S2 into a tubular furnace and heat it to 900°C at a rate of 9°C / min for vacuum annealing. Keep it warm for two hours and then cool it down naturally. During the vacuum annealing process, use plasma diagnostic technology to control the O2 introduced into the tubular furnace so that its flow rate is 10sccm. After the annealing is completed, the film preparation is completed.
[0036] Example 2
[0037] This embodiment provides a method for preparing a Y2O3 thin film with compactness and etching resistance. The steps are basically the same as those in Embodiment 1, except that the substrate material in step S1 is replaced with AlN, and the rest remain unchanged.
[0038] Example 3
[0039] This embodiment provides a method for preparing a Y2O3 thin film with compactness and etching resistance. The steps are basically the same as those in Example 1, except that the substrate material in step S1 is replaced with SiC, and the rest remain unchanged.
[0040] Example 4
[0041] This embodiment provides a method for preparing a Y2O3 thin film with compactness and etching resistance. The steps are basically the same as those in Embodiment 1, except that the substrate material in step S1 is replaced with Al, and the rest remain unchanged.
[0042] Example 5
[0043] This embodiment provides a method for preparing a Y2O3 thin film with compactness and etching resistance. The steps are basically the same as those in Example 1, except that the substrate material in step S1 is replaced with quartz, and the rest remain unchanged.
[0044] Example 6
[0045] This embodiment provides a method for preparing a Y2O3 thin film with compactness and etching resistance. The steps are basically the same as those in Example 1, except that the vacuum annealing in step S3 is changed to 800°C, the O2 flow rate is 15sccm, and the rest remain unchanged.
[0046] Example 7
[0047] This embodiment provides a method for preparing a Y2O3 thin film with compactness and etching resistance. The steps are basically the same as those in Example 1, except that the vacuum annealing in step S3 is changed to 1000°C, the O2 flow rate is 5sccm, and the rest remain unchanged.
[0048] Comparative Example 1
[0049] This comparative example provides a method for preparing a Y2O3 film with compactness and etching resistance, and its steps are basically the same as those of Example 1, except that the vacuum annealing in step S3 is changed to conventional annealing in air, and the rest remain unchanged.
[0050] Comparative Example 2
[0051] This comparative example provides a method for preparing a Y2O3 thin film with compactness and etching resistance. The steps are basically the same as those in Example 1, except that the vacuum annealing temperature in step S3 is changed from 900°C to 600°C, and the rest remain unchanged.
[0052] Comparative Example 3
[0053] This comparative example provides a method for preparing a Y2O3 thin film with compactness and etching resistance. The steps are basically the same as those in Example 1, except that O2 is not introduced during the vacuum annealing process in step S3, and the rest remain unchanged.
[0054] Comparative Example 4
[0055] This comparative example provides a method for preparing a Y2O3 thin film with compactness and etching resistance. The steps are basically the same as those in Example 1, except that the vacuum annealing temperature in step S3 is changed from 900°C to 600°C, and O2 is not introduced, while the rest remain unchanged.
[0056] Comparative Example 5
[0057] This comparative example provides a method for preparing a Y2O3 thin film with compactness and etching resistance. The steps are basically the same as those in Example 1, except that the vacuum annealing temperature in step S3 is changed from 900°C to 300°C, and O2 is not introduced, while the rest remain unchanged.
[0058] Comparative Example 6
[0059] This comparative example provides a method for preparing a Y2O3 thin film with compactness and etching resistance, and its steps are basically the same as those of Example 1, except that: in step S1, the process of treating the substrate with a UV light cleaning machine is omitted, and the rest remains unchanged.
[0060] Furthermore, in order to understand the appearance, performance, etc. of the Y2O3 thin films prepared in the above-mentioned embodiments and comparative examples, the following experiments were also conducted.
[0061] Y2O3 film etching resistance detection steps: put the prepared Y2O3 films into ICP inductively coupled plasma etching equipment in turn, and use Ar and O2 mixed gas to clean the inside of the etcher chamber after vacuuming to remove impurities and etching residues in the chamber; after cleaning, introduce CF4 and O2, adjust the coil power to 800W, the bias power to 100W, and the chamber pressure to 15mTorr, and chemically etch the film for 40min; after etching, take out the film and detect the etching rate with a step profiler. The results are shown in Table 1.
[0062] Table 1 Etching rate of various Y2O3 films
[0063]
[0064] It can be seen from Table 1 that compared with ordinary air annealing, the ultra-high temperature vacuum annealing treatment of the Y2O3 film and the oxygen plasma technology significantly reduced the film etching rate, and the Y2O3 film etching rate after treatment was maintained within 1.5nm / min. Comparing Example 1 with Comparative Example 1, it was found that the etching rate of the Y2O3 film after ozone treatment was lower.
[0065] Figure 1 The following are the sample images of Y2O3 on (a) Si, (b) AlN, (c) SiC, (d) Al, and (e) quartz substrates in Examples 1 to 5. It can be seen from the figure that the Y2O3 film appears black on Si, AlN, and SiC substrates, and appears yellow-brown on bright substrates such as Al and quartz, and the film has a uniform gloss.
[0066] Figure 2The following is a comparison of the Si wafer in Example 1 before (a) and after (b) ozone treatment in a UV light cleaning machine. It can be seen from the figure that after ozone treatment, the organic matter and impurities on the surface of the Si wafer are removed, and the surface of the Si wafer is very clean, which is conducive to improving the adhesion between the film and the substrate, making the combination more firm; at the same time, the clean substrate will also avoid the introduction of foreign pollutants during the film deposition process, reduce defects in the film preparation process, and make the etching rate of Example 1 lower than that of Comparative Example 6.
[0067] Figure 3 The XRD diffraction patterns of the films formed by vacuum annealing of Y2O3 on (a) Si, (b) AlN, (c) SiC, (d) Al, and (e) quartz substrates at 900°C and O2, respectively, and the films formed by vacuum annealing of Y2O3 on Si at (f) 900°C air annealing, (g) 600°C vacuum annealing, and (h) 300°C vacuum annealing in O2 in the comparative example. It can be seen from the figure that the annealed Y2O3 film is a cubic phase with preferred orientations of (222), (400), (440), and (622) crystal planes. The crystals with a body-centered cubic structure have better advantages in hardness and chemical stability, so that the Y2O3 film has better etching resistance.
[0068] Figure 4 Surface SEM images of (a) Example 1 and (b) Comparative Example 1. Figure 4 (a) shows that after vacuum annealing with O2, the grains of the Y2O3 film are arranged in irregular polygons, tightly packed, without holes, oxygen vacancies and defects, and have good compactness. Figure 4 As can be seen in (b), the grains of the Y2O3 film after air annealing are arranged loosely, the pores between the grains are large, and the density of the film is poor.
[0069] In summary, the method provided by the present invention can prepare Y2O3 thin films with high density and excellent etching resistance on different substrates. By using a UV light cleaning machine to process the substrate, using magnetron sputtering and supplemented by an improved post-annealing process, O2 is introduced during the ultra-high temperature annealing process under vacuum to improve the microstructure of the film, reduce the structural defects of the film, and increase the density of the film, thereby achieving the purpose of enhancing the etching resistance of the film, effectively extending the service life of the material inside the etcher cavity while reducing the pollution caused by etching.
[0070] The specific raw materials not described in the present invention are all existing materials and can be directly purchased from the market.
[0071] The above are only preferred embodiments of the present invention and are not intended to limit the protection scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a Y2O3 thin film having compactness and etching resistance, characterized in that: The following steps are involved: S1. Clean the substrate, blow dry it, and place it in a UV light cleaning machine for activation treatment; S2, placing the substrate in step S1 in a magnetron sputtering coating machine, evacuating and heating at the same time, introducing argon gas after reaching the background vacuum, pre-sputtering the Y2O3 target material, opening the baffle after the pre-sputtering is completed, adjusting the chamber pressure, and formally starting sputtering, and taking out the substrate after sputtering is completed; S3, vacuum annealing the substrate in step S2 at 800-1000°C, continuously introducing O2 during the annealing process, and naturally cooling the substrate in a vacuum environment after the annealing is completed, thereby completing the preparation of the Y2O3 thin film; The background vacuum in step S2 is 10 -4 Pa, the heating is such that the substrate temperature is 200° C. to 300° C., and the argon gas flow rate is 40 sccm to 100 sccm; The sputtering powers of the pre-sputtering and the formal sputtering in step S2 are both 100-180W; wherein the pre-sputtering time is 3-8min, and the formal sputtering time is 300-400min; and the gas pressure in the chamber during the formal sputtering is 0.6Pa; In the annealing process in step S3, the heating rate is 8-10°C / min and the holding time is 2-3h; The O2 flow rate in step S3 is 5-15 sccm.
2. The method according to claim 1, characterized in that In step S1, the substrate material includes Si, AlN, SiC, Al, and quartz.
3. The method according to claim 1, characterized in that The cleaning in step S1 is performed by using acetone, alcohol and deionized water in sequence for 10 to 20 minutes; the drying is performed by using nitrogen.
4. The method according to claim 1, characterized in that: The UV light cleaning machine in step S1 emits ultraviolet light with a wavelength of 185 nm and an activation time of 18 to 22 minutes.
5. The method according to any one of claims 1 to 4, characterized in that: The Y2O3 film has a thickness of ≥1 μm.