A high performance powder metallurgy oil-containing bearing and a manufacturing method thereof

By using B4C, V2O5 and SiO2 in the bearings to enhance iron powder and pickle treatment, combined with bio-based adhesives and modified vegetable oil grease, the performance problems of vegetable oil-based grease under oxidation and temperature increase are solved, and lubrication is achieved The stability of performance and the wear resistance of bearings are improved.

CN118527659BActive Publication Date: 2024-11-22烟台东星大韩粉末冶金有限公司
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410970785.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-22
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

Vegetable oil-based greases are prone to deterioration under oxidation, resulting in a decrease in lubricating performance. The increase in ambient temperature during continuous operation of the machinery leads to a decrease in viscosity, resulting in a decrease in lubricating performance and grease leakage.

Method used

B4C, V2O5 and SiO2 are used as reinforcement powder to enhance the iron powder. The inner and outer rings of the bearing are prepared by pressing and sintering, and acid is injected between the inner ring and the outer ring for pickling to improve the surface roughness, and then assemble and Inject bio-based adhesives and modified vegetable oil grease to prevent grease displacement and leakage.

Benefits of technology

The stability of lubricating performance is achieved, the leakage and maintenance requirements of grease are avoided, and the wear resistance and operation stability of bearings are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118527659B_ABST
    Figure CN118527659B_ABST
Patent Text Reader

Abstract

The present invention relates to a high-performance powder metallurgy oil-containing bearing and a manufacturing method thereof, belonging to the technical field of metal powder processing, using B4C, V2O5 and SiO2 as reinforcing powder to reinforce iron powder, then placing it in a mold for pressing and sintering, preparing the inner ring and outer ring of the bearing, using a dust cover to seal the inner ring and outer ring, injecting acid into the inner cavity to pickle the inner cavity, and improving the surface roughness of the inner part of the bearing, and then assembling the inner ring, outer ring, steel ball and retainer, injecting bio-based adhesive and grease in turn, and resealing the dust cover to prepare a high-performance powder metallurgy oil-containing bearing. The manufactured bearing avoids the use of petroleum-based lubricants, and can play a good protective role on components, has stable lubrication performance, avoids displacement and leakage of grease, and reduces the maintenance required for the bearing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal powder processing, in particular to a high-performance powder metallurgy oil-containing bearing and a manufacturing method thereof. Background Art

[0002] Oil-containing bearings are sliding bearings made by sintering and pressing metal powder, which contain grease inside. This type of bearing has the characteristics of high wear resistance, low friction coefficient, good self-lubricating performance, high compressive strength and good fatigue resistance, and is widely used in the automotive industry, aerospace and other fields.

[0003] In recent years, as people's environmental awareness has been further improved, more and more manufacturers have chosen to use green and environmentally friendly biodegradable lubricating products in bearings in order to avoid environmental pollution caused by using petroleum-based grease in bearings. Among them, vegetable oil-based grease is the most commonly used category of green grease. In addition to being non-toxic and having good degradation performance, vegetable oil molecules can form an adsorption film on the metal surface, and the fatty acids in it can react with the metal surface to form a single layer of metal soap film, which can reduce friction and anti-wear, and provide effective lubrication protection for bearings.

[0004] However, vegetable oil grease is prone to deterioration under oxidation, and may produce precipitation and acidic substances, which will reduce its lubrication performance and the protection effect on parts. In addition, due to the narrow kinematic viscosity range of vegetable oil grease, when the machine is working continuously, the working environment temperature of vegetable oil grease rises, which can easily lead to a decrease in viscosity, resulting in a decrease in lubrication performance and grease leakage.

[0005] Therefore, a new preparation process for oil-containing bearings is needed to improve the compatibility between bearings and grease and improve the wear resistance of bearings. Summary of the invention

[0006] The purpose of the present invention is to provide a high-performance powder metallurgy oil-containing bearing and a method for making the same, so as to solve the problems raised in the background technology. B4C, V2O5 and SiO2 are used as reinforcing powders to reinforce iron powder, which is then placed in a mold for pressing and sintering to prepare the inner and outer rings of the bearing. After the inner and outer rings are sealed with a dust cover, acid is injected into the inner cavity to pickle the inner cavity to increase the surface roughness of the inner part of the bearing. Subsequently, the inner ring, outer ring, steel ball and retainer are assembled, and bio-based adhesives and grease are injected in turn. After the dust cover is resealed, a high-performance powder metallurgy oil-containing bearing is prepared. The bearings prepared avoid the use of petroleum-based lubricants, and can provide good protection for components. The lubrication performance is stable, the displacement and leakage of grease is avoided, and the maintenance required for the bearing is reduced.

[0007] To achieve the above object, the present invention provides the following technical solutions:

[0008] A method for manufacturing a high-performance powder metallurgy oil-containing bearing comprises the following steps:

[0009] S1, placing iron powder and reinforcing powder in a mixer and stirring to obtain base powder, wherein the amount of reinforcing powder used is 1-3wt% of the iron powder;

[0010] S2, then adding the base powder into the inner ring and outer ring pressing molds to press into blanks, the pressure during the pressing process is 300-450Mpa, the pressing time is 5-20 minutes, and the primary blanks are obtained respectively;

[0011] S3, vacuum sintering the blank obtained in step S2: setting the vacuum degree to 1.3×10 -3 Pa, raising the temperature in the furnace to 200-300°C for pre-sintering for 10-15 minutes; then raising the temperature to 700-750°C at a heating rate of 10-20°C / min, treating for 20-30 minutes, and then naturally cooling to room temperature to obtain a sintered blank;

[0012] S4, demoulding the sintered blank, treating the outer surface of the inner ring and the inner surface of the outer ring with acid, then washing with clean water, drying and placing in a vacuum oil immersion machine for vacuum oil immersion, the vacuum degree is 1.5×10 -3 -3×10 -3 pa, the oil temperature is 40-80℃, and the inner ring and the outer ring are obtained; then the inner ring, the outer ring, the steel ball and the retainer are assembled, and the bio-based adhesive is injected between the inner ring and the outer ring. After the coating is complete, grease is injected, and then a dust cover is used for sealing to obtain a high-performance powder metallurgy oil-containing bearing.

[0013] Further, the lubricating grease is prepared by the following steps:

[0014] A1. Stir vegetable oil, dodecane and sodium hydroxide methanol solution at room temperature until uniform, then raise the system temperature to 80°C, add boron trifluoride methanol solution after treating for 0.5-2 hours, raise the temperature to 80-120°C, treat for 10-30 minutes, then add n-heptane for 3-5 minutes, wash the system, stand and separate, and retain the upper liquid to obtain esterified vegetable oil;

[0015] A2, adding ethanolamine to the esterified vegetable oil obtained in step A1, stirring at room temperature for 5-10 minutes, adding sodium methoxide solution for 3-5 minutes and raising the system temperature to 50-70°C, reacting for 4-5 hours, transferring the system to dichloromethane, washing the system and drying to obtain modified vegetable oil;

[0016] A3. Add microcrystalline wax to the modified vegetable oil in step A2, raise the temperature to 80-100°C, stir at 30-60 rpm for 15-30 minutes, and then let gel stand at 20°C for 24 hours to obtain grease.

[0017] Further, the lubricating grease is prepared by the following steps:

[0018] A1. Stir vegetable oil, dodecane and a freshly prepared 0.5 mol / L sodium hydroxide methanol solution at room temperature until uniform, then raise the system temperature to 80°C, add boron trifluoride methanol solution after treating for 0.5-2 hours, raise the temperature to 100°C, treat for 10-30 minutes, continue to add n-heptane, treat for 3-5 minutes, wash the system with a saturated sodium chloride solution, let stand and separate, and retain the upper liquid to obtain esterified vegetable oil;

[0019] In the above reaction process, dodecane is used as a catalyst and system diluent, and then a sodium hydroxide methanol solution reacts with the vegetable oil. The vegetable oil first undergoes a saponification reaction in an alkaline environment and then undergoes an esterification reaction with methanol to generate fatty acid esters. n-heptane is added as an extractant to promote the stratification of the esters to obtain esterified vegetable oil.

[0020] A2, adding ethanolamine to the esterified vegetable oil obtained in step A1, stirring at room temperature for 5-10 minutes, adding 0.05 mol / L sodium methoxide solution for 3-5 minutes and raising the system temperature to 60°C, reacting for 4-5 hours, transferring the system to dichloromethane, washing the system with saturated brine and drying with a desiccant, and removing the solvent by evaporation under reduced pressure to obtain a modified vegetable oil;

[0021] In the above reaction process, ethanolamine is used as an amidation agent to react with the ester group in the esterified vegetable oil to generate an amide bond, thereby introducing an amide functional group into the vegetable oil system to obtain a modified vegetable oil.

[0022] A3. Add microcrystalline wax to the modified vegetable oil in step A2, raise the temperature to 80-100°C, stir at 30-60 rpm for 15-30 minutes, and then let gel stand at 20°C for 24 hours to obtain grease.

[0023] Furthermore, the mass ratio of vegetable oil, ethanolamine and microcrystalline wax is 300:(50-100):(9-80).

[0024] Further, the bio-based adhesive is prepared by the following steps:

[0025] B1, adding 2-morpholineethanesulfonic acid solution and NaCl solution into sterile deionized water, adjusting the pH value of the system to 5.1, and obtaining 2-morpholineethanesulfonic acid buffer for standby use;

[0026] B2. Dissolve carboxymethyl cellulose, EDC, N-hydroxysuccinimide and dopamine hydrochloride in 2-morpholineethanesulfonic acid buffer, stir well for 12-48 hours at room temperature under an inert gas atmosphere, then freeze-dry in a freeze dryer, and then resuspend in deionized water to obtain a bio-based adhesive.

[0027] In the above reaction process, in the EDC / NHS environment, the carboxyl groups on the carboxymethyl cellulose react with the amino groups on the dopamine hydrochloride to form amide bonds, thereby preparing a bio-based adhesive.

[0028] Furthermore, in step B2, the mass ratio of carboxymethyl cellulose to dopamine hydrochloride is (3-6):(0.5-1.5).

[0029] Further, in step S4, the specific operation of the acid treatment is:

[0030] Wash the surface of the inner ring and outer ring with anhydrous ethanol respectively, then install the dust cover, inject the acid into the sealed cavity formed by the inner ring, outer ring and dust cover, and treat it for 10-30 minutes after filling, then remove the dust cover and rinse the sealed cavity with anhydrous ethanol.

[0031] Furthermore, the acid solution is a 5-10wt% sulfuric acid solution.

[0032] Furthermore, in step S4, the steel ball is at least one of carbon steel, chrome steel ball, and stainless steel ball, and the material of the dust cover is at least one of fluorinated rubber, polytetrafluoroethylene, ethylene propylene rubber, fluorosilicone rubber, polyurethane, and chloroprene rubber.

[0033] Furthermore, in step S1, the reinforcing powder is obtained by mixing B4C, V2O5 and SiO2 in a mass ratio of (1-2):(1-2):(2-4), wherein the particle sizes of B4C and V2O5 are 0-50 μm, and the particle size of SiO2 is 0-20 nm.

[0034] A high-performance powder metallurgy oil-containing bearing comprises an inner ring, an outer ring, steel balls, a retainer and a dust cover, wherein grease is provided between the inner ring and the outer ring and the grease is sealed by the dust cover.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] In the technical solution of the present invention, B4C, V2O5 and SiO2 are used as reinforcing powders to reinforce iron powder, which is then placed in a mold for pressing and sintering to prepare the inner and outer rings of the bearing. After the inner and outer rings are sealed with a dust cover, acid is injected into them to pickle the internal cavity to increase the surface roughness of the bearing. Subsequently, the inner and outer rings, steel balls and retainers are assembled, and bio-based adhesives and grease are injected in sequence. After the dust cover is resealed, a high-performance powder metallurgy oil-containing bearing is prepared. The bearings prepared avoid the use of petroleum-based lubricants, and can provide good protection for components. The lubrication performance is stable, the displacement and leakage of grease is avoided, and the maintenance required for the bearings is reduced.

[0037] In the technical solution of the present invention, impurities such as free fatty acids and glycerides in the vegetable oil are removed by water and alkali treatment, and then the vegetable oil is esterified and amidated by amino alcohol, so that amide groups are introduced into the vegetable oil, the content of polar groups in the vegetable oil is increased, and the cross-linking of the vegetable oil is promoted, and the grease is made in the form of a gel. During the operation of the bearing, the grease is subjected to shear force to destroy a part of the gel network, releasing the vegetable oil. After the shear stops, the intermolecular hydrogen bonds can re-drive the self-assembly of the gel factor to capture the vegetable oil and the oil that penetrates the bearing during operation, thereby avoiding the creep and leakage of the grease.

[0038] In the technical solution of the present invention, carboxylated cellulose is modified by using dopamine hydrochloride to prepare a modified carboxylated cellulose solution, which is used as a bio-based adhesive and is used for the treatment of the inner ring and the outer ring. The bio-based adhesive interacts with the metal components of the inner ring and the outer ring to produce metal ion coordination bonds, and can be well attached to the metal wall material. The amide group contained in the bio-based adhesive can produce a good blending effect with the grease, and with the slow oxidation of air, the catechol group on the dopamine hydrochloride in the bio-based adhesive is converted into catechol quinone, which avoids the oxidation and deterioration of vegetable oil during the operation of the bearing to produce precipitation and cause wear to the bearing. In addition, after the inner ring and the outer ring of the bearing are pickled, the surface of the material becomes rough, which can improve the adhesion effect of the adhesive, prevent grease leakage, and improve the operation stability of the bearing. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0040] Figure 1 The present invention is a schematic structural diagram of a high-performance powder metallurgy oil-containing bearing and a manufacturing method thereof, wherein the bearing is manufactured.

[0041] Reference numerals: steel ball 1; retainer 2; inner ring 3; dust cover 4; outer ring 5; grease 6. DETAILED DESCRIPTION

[0042] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0043] In the following embodiments and comparative examples, the vacuum oil used in the vacuum oil immersion machine is V100 engine oil, the vegetable oil used is process palm oil, the dust cover 4 used is made of fluorinated rubber, the model of the bearing obtained is 62212, and the specific dimensions are: the nominal inner diameter is 60 mm, the outer diameter is 110 mm, and the width is 28 mm.

[0044] Embodiment 1: A high-performance powder metallurgy oil-containing bearing comprises an inner ring 3, an outer ring 5, a steel ball 1, a retainer 2 and a dust cover 4, wherein there is grease 6 between the inner ring 3 and the outer ring 5, and the grease 6 is sealed by the dust cover 4.

[0045] A method for manufacturing a high-performance powder metallurgy oil-containing bearing comprises the following steps:

[0046] S1. Mix B4C, V2O5 and SiO2 in a mass ratio of 1:1:2 to obtain a reinforced powder, wherein the particle size of B4C and V2O5 is 0-50 μm, and the particle size of SiO2 is 0-20 nm;

[0047] Then, the iron powder and the reinforcing powder were placed in a mixer and stirred at a rate of 15 rpm for 20 minutes to obtain a base powder, wherein the amount of the reinforcing powder used was 1 wt % of the iron powder;

[0048] S2, then add the base powder into the inner ring 3 and the outer ring 5 pressing molds to press into blanks, the pressure during the pressing process is 300 MPa, the pressing time is 5 minutes, and the primary blanks are obtained respectively;

[0049] S3, vacuum sintering the blank obtained in step S2: setting the vacuum degree to 1.3×10 -3 Pa, raising the temperature in the furnace to 200°C for pre-sintering for 10 minutes; then raising the temperature to 700°C at a heating rate of 10°C / min, treating for 20 minutes, and naturally cooling to room temperature to obtain a sintered blank;

[0050] S4, demould the sintered blank, wash the surface of the inner ring 3 and the outer ring 5 with anhydrous ethanol, then install the dust cover 4, inject 5wt% sulfuric acid solution into the sealed cavity formed by the inner ring 3, the outer ring 5 and the dust cover 4, fill it up and treat it for 10 minutes, then remove the dust cover 4 and rinse the sealed cavity with anhydrous ethanol, then wash it with clean water, dry it, and place it in a vacuum oil immersion machine for vacuum oil immersion, and the vacuum degree is 1.5×10 -3 pa, the oil temperature is 40°C, and an inner ring 3 and an outer ring 5 are obtained; then the inner ring 3, the outer ring 5, the steel ball 1 and the retainer 2 are assembled, 20 mL of bio-based adhesive is injected between the inner ring 3 and the outer ring 5, and 50 mL of grease 6 is injected after the coating is complete, and then a dust cover 4 is used for sealing, so as to obtain a high-performance powder metallurgy oil-containing bearing;

[0051] Wherein, lubricating grease 6 is prepared by following steps:

[0052] A1. Weigh 300 mg of vegetable oil, 100 mg of dodecane and 8 mL of freshly prepared 0.5 mol / L sodium hydroxide methanol solution and stir them at room temperature until they are uniform. Then, raise the system temperature to 80° C., add 7 mL of boron trifluoride methanol solution after treating for 0.5 hour, raise the temperature to 100° C., treat for 10 minutes, then continue to add 5 mL of n-heptane, treat for 3 minutes, wash the system with 20 mL of saturated sodium chloride solution, let stand for stratification, and retain the upper liquid to obtain esterified vegetable oil;

[0053] A2. Add 50 mg of ethanolamine to the esterified vegetable oil obtained in step A1, stir at room temperature for 5 minutes, add 0.45 ml of 0.05 mol / L sodium methoxide solution and raise the system temperature to 60°C. After reacting for 4 hours, transfer the system to dichloromethane, wash the system with 20 mL of saturated brine, dry with anhydrous magnesium sulfate, and remove the solvent by evaporation under reduced pressure to obtain modified vegetable oil;

[0054] A3, adding 9 mg of microcrystalline wax to the modified vegetable oil in step A2, raising the temperature to 80°C and stirring at 30 rpm for 15 minutes, and then leaving the gel at 20°C for 24 hours to obtain grease 6;

[0055] Wherein, the bio-based adhesive is prepared by the following steps:

[0056] B1, add 0.585g 0.1mol / L 2-morpholineethanesulfonic acid solution and 0.0876g 0.05mol / L NaCl solution to 30mL sterile deionized water, adjust the pH value of the system to 5.1 with NaOH solution, and obtain 2-morpholineethanesulfonic acid buffer for standby use;

[0057] B2. Take 30 mL of the 2-morpholineethanesulfonic acid buffer prepared in step B1, add 3 g of carboxymethyl cellulose, 0.192 g of EDC, 0.115 g of N-hydroxysuccinimide and 0.5 g of dopamine hydrochloride, stir well for 12 hours at room temperature and nitrogen atmosphere, then freeze-dry in a freeze dryer, and then resuspend in 30 mL of deionized water to obtain a bio-based adhesive.

[0058] Embodiment 2: A high-performance powder metallurgy oil-containing bearing comprises an inner ring 3, an outer ring 5, a steel ball 1, a retainer 2 and a dust cover 4, wherein there is grease 6 between the inner ring 3 and the outer ring 5, and the grease 6 is sealed by the dust cover 4.

[0059] A method for manufacturing a high-performance powder metallurgy oil-containing bearing comprises the following steps:

[0060] S1. Mix B4C, V2O5 and SiO2 in a mass ratio of 1:1:3 to obtain a reinforced powder, wherein the particle sizes of B4C and V2O5 are 0-50 μm, and the particle size of SiO2 is 0-20 nm;

[0061] The iron powder and the reinforcing powder were placed in a mixer and stirred at a rate of 15 rpm for 30 minutes to obtain a base powder, wherein the amount of the reinforcing powder used was 2 wt % of the iron powder;

[0062] S2, then add the base powder into the inner ring 3 and the outer ring 5 pressing molds to press into blanks, the pressure during the pressing process is 400Mpa, the pressing time is 10 minutes, and the primary blanks are obtained respectively;

[0063] S3, vacuum sintering the blank obtained in step S2: setting the vacuum degree to 1.3×10 -3 Pa, raising the temperature in the furnace to 250°C for pre-sintering for 15 minutes; then raising the temperature to 720°C at a heating rate of 20°C / min, treating for 30 minutes, and naturally cooling to room temperature to obtain a sintered blank;

[0064] S4, demould the sintered blank, wash the surface of the inner ring 3 and the outer ring 5 with anhydrous ethanol, then install the dust cover 4, inject 8wt% sulfuric acid solution into the sealed cavity formed by the inner ring 3, the outer ring 5 and the dust cover 4, and treat it for 20 minutes after filling, then remove the dust cover 4 and rinse the sealed cavity with anhydrous ethanol, then wash it with clean water, dry it, and place it in a vacuum oil immersion machine for vacuum oil immersion, and the vacuum degree is 2×10 -3 pa, the oil temperature is 60°C, and an inner ring 3 and an outer ring 5 are obtained; then the inner ring 3, the outer ring 5, the steel ball 1 and the retainer 2 are assembled, 20 mL of bio-based adhesive is injected between the inner ring 3 and the outer ring 5, and 50 mL of grease 6 is injected after the coating is complete, and then a dust cover 4 is used for sealing, so as to obtain a high-performance powder metallurgy oil-containing bearing;

[0065] Wherein, lubricating grease 6 is prepared by following steps:

[0066] A1. Weigh 300 mg of vegetable oil, 100 mg of dodecane and 8 mL of freshly prepared 0.5 mol / L sodium hydroxide methanol solution and stir them at room temperature until they are uniform. Then, raise the system temperature to 80° C., add 7 mL of boron trifluoride methanol solution after treating for 1 hour, raise the temperature to 100° C., treat for 20 minutes, then continue to add 5 mL of n-heptane, treat for 4 minutes, wash the system with 20 mL of saturated sodium chloride solution, let stand for stratification, and retain the upper layer of liquid to obtain esterified vegetable oil.

[0067] A2. Add 80 mg of ethanolamine to the esterified vegetable oil obtained in step A1, stir at room temperature for 8 minutes, add 0.45 ml of 0.05 mol / L sodium methoxide solution and raise the system temperature to 60°C. After reacting for 5 hours, transfer the system to dichloromethane, wash the system with 20 mL of saturated brine, dry with anhydrous magnesium sulfate, and evaporate under reduced pressure to remove the solvent to obtain modified vegetable oil;

[0068] A3, adding 40 mg of microcrystalline wax to the modified vegetable oil in step A2, raising the temperature to 90°C and stirring at 60 rpm for 20 minutes, then leaving the gel at 20°C for 24 hours to obtain grease 6;

[0069] Wherein, the bio-based adhesive is prepared by the following steps:

[0070] B1, add 0.585g 0.1mol / L 2-morpholineethanesulfonic acid solution and 0.0876g 0.05mol / L NaCl solution to 30mL sterile deionized water, adjust the pH value of the system to 5.1 with NaOH solution, and obtain 2-morpholineethanesulfonic acid buffer for standby use;

[0071] B2. Take 30 mL of the 2-morpholineethanesulfonic acid buffer prepared in step B1, add 5 g of carboxymethyl cellulose, 0.192 g of EDC, 0.115 g of N-hydroxysuccinimide and 1 g of dopamine hydrochloride, stir well for 24 hours at room temperature and nitrogen atmosphere, then freeze-dry in a freeze dryer, and then resuspend in 30 mL of deionized water to obtain a biobased adhesive.

[0072] Embodiment 3: A high-performance powder metallurgy oil-containing bearing comprises an inner ring 3, an outer ring 5, a steel ball 1, a retainer 2 and a dust cover 4, wherein there is grease 6 between the inner ring 3 and the outer ring 5, and the grease 6 is sealed by the dust cover 4.

[0073] A method for manufacturing a high-performance powder metallurgy oil-containing bearing comprises the following steps:

[0074] S1. Mix B4C, V2O5 and SiO2 in a mass ratio of 2:2:4 to obtain a reinforced powder, wherein the particle sizes of B4C and V2O5 are 0-50 μm, and the particle size of SiO2 is 0-20 nm;

[0075] The iron powder and the reinforcing powder were placed in a mixer and stirred at a rate of 30 rpm for 30 minutes to obtain a base powder, wherein the amount of the reinforcing powder used was 3 wt % of the iron powder;

[0076] S2, then add the base powder into the inner ring 3 and the outer ring 5 pressing molds to press into blanks, the pressure during the pressing process is 450 MPa, the pressing time is 20 minutes, and the primary blanks are obtained respectively;

[0077] S3, vacuum sintering the blank obtained in step S2: setting the vacuum degree to 1.3×10 -3 Pa, raise the temperature in the furnace to 300°C for pre-sintering for 15 minutes; then raise the temperature to 750°C at a heating rate of 20°C / min, treat for 30 minutes, and naturally cool to room temperature to obtain a sintered blank;

[0078] S4, demould and remove the sintered blank, wash the surface of the inner ring 3 and the outer ring 5 with anhydrous ethanol respectively, then install the dust cover 4, inject 10wt% sulfuric acid solution into the sealed cavity formed by the inner ring 3, the outer ring 5 and the dust cover 4, fill it up and treat it for 30 minutes, then remove the dust cover 4 and rinse the sealed cavity with anhydrous ethanol, then wash it with clean water, dry it and place it in a vacuum oil immersion machine for vacuum oil immersion, and the vacuum degree is 3×10 -3 pa, the oil temperature is 80°C, and an inner ring 3 and an outer ring 5 are obtained; then the inner ring 3, the outer ring 5, the steel ball 1 and the retainer 2 are assembled, 20 mL of bio-based adhesive is injected between the inner ring 3 and the outer ring 5, and 50 mL of grease 6 is injected after the coating is complete, and then a dust cover 4 is used for sealing, so as to obtain a high-performance powder metallurgy oil-containing bearing;

[0079] Wherein, lubricating grease 6 is prepared by following steps:

[0080] A1. Weigh 300 mg of vegetable oil, 100 mg of dodecane and 8 mL of freshly prepared 0.5 mol / L sodium hydroxide methanol solution and stir them at room temperature until they are uniform. Then, raise the system temperature to 80° C., add 7 mL of boron trifluoride methanol solution after treating for 2 hours, raise the temperature to 100° C., treat for 30 minutes, then continue to add 5 mL of n-heptane, treat for 5 minutes, wash the system with 20 mL of saturated sodium chloride solution, let stand for stratification, and retain the upper liquid to obtain esterified vegetable oil.

[0081] A2. Add 100 mg of ethanolamine to the esterified vegetable oil obtained in step A1, stir at room temperature for 10 minutes, add 0.45 ml of 0.05 mol / L sodium methoxide solution and raise the system temperature to 60°C. After reacting for 5 hours, transfer the system to dichloromethane, wash the system with 20 mL of saturated brine and dry it with anhydrous magnesium sulfate, and evaporate under reduced pressure to remove the solvent to obtain modified vegetable oil;

[0082] A3, adding 80 mg of microcrystalline wax to the modified vegetable oil in step A2, raising the temperature to 100°C and stirring at 60 rpm for 30 minutes, then leaving the gel at 20°C for 24 hours to obtain grease 6;

[0083] Wherein, the bio-based adhesive is prepared by the following steps:

[0084] B1, add 0.585g 0.1mol / L 2-morpholineethanesulfonic acid solution and 0.0876g 0.05mol / L NaCl solution to 30mL sterile deionized water, adjust the pH value of the system to 5.1 with NaOH solution, and obtain 2-morpholineethanesulfonic acid buffer for standby use;

[0085] B2. Take 30 mL of the 2-morpholineethanesulfonic acid buffer prepared in step B1, add 6 g of carboxymethyl cellulose, 0.192 g of EDC, 0.115 g of N-hydroxysuccinimide and 1.5 g of dopamine hydrochloride, stir well at room temperature and nitrogen atmosphere for 48 hours, then freeze-dry in a freeze dryer, and then resuspend in 30 mL of deionized water to obtain a bio-based adhesive.

[0086] Comparative Example 1: A high-performance powder metallurgy oil-containing bearing, comprising an inner ring 3, an outer ring 5, a steel ball 1, a retainer 2 and a dust cover 4, with grease 6 between the inner ring 3 and the outer ring 5, and the grease 6 is sealed by the dust cover 4.

[0087] A method for manufacturing a high-performance powder metallurgy oil-containing bearing comprises the following steps:

[0088] S1. Mix B4C, V2O5 and SiO2 in a mass ratio of 1:1:2 to obtain a reinforced powder, wherein the particle size of B4C and V2O5 is 0-50 μm, and the particle size of SiO2 is 0-20 nm;

[0089] Then, the iron powder and the reinforcing powder were placed in a mixer and stirred at a rate of 15 rpm for 20 minutes to obtain a base powder, wherein the amount of the reinforcing powder used was 1 wt % of the iron powder;

[0090] S2, then add the base powder into the inner ring 3 and the outer ring 5 pressing molds to press into blanks, the pressure during the pressing process is 300 MPa, the pressing time is 5 minutes, and the primary blanks are obtained respectively;

[0091] S3, vacuum sintering the blank obtained in step S2: setting the vacuum degree to 1.3×10 -3 Pa, raising the temperature in the furnace to 200°C for pre-sintering for 10 minutes; then raising the temperature to 700°C at a heating rate of 10°C / min, treating for 20 minutes, and naturally cooling to room temperature to obtain a sintered blank;

[0092] S4, the sintered blank is demoulded and taken out, and then placed in a vacuum oil impregnation machine for vacuum oil impregnation, with a vacuum degree of 1.5×10 - 3 pa, the oil temperature is 40°C, and an inner ring 3 and an outer ring 5 are obtained; then the inner ring 3, the outer ring 5, the steel ball 1 and the retainer 2 are assembled, 20 mL of bio-based adhesive is injected between the inner ring 3 and the outer ring 5, and 50 mL of grease 6 is injected after the coating is complete, and then a dust cover 4 is used for sealing, so as to obtain a high-performance powder metallurgy oil-containing bearing;

[0093] Wherein, lubricating grease 6 is prepared by following steps:

[0094] A1. Weigh 300 mg of vegetable oil, 100 mg of dodecane and 8 mL of freshly prepared 0.5 mol / L sodium hydroxide methanol solution and stir them at room temperature until they are uniform. Then, raise the system temperature to 80° C., add 7 mL of boron trifluoride methanol solution after treating for 0.5 hour, raise the temperature to 100° C., treat for 10 minutes, then continue to add 5 mL of n-heptane, treat for 3 minutes, wash the system with 20 mL of saturated sodium chloride solution, let stand for stratification, and retain the upper liquid to obtain esterified vegetable oil;

[0095] A2. Add 50 mg of ethanolamine to the esterified vegetable oil obtained in step A1, stir at room temperature for 5 minutes, add 0.45 ml of 0.05 mol / L sodium methoxide solution and raise the system temperature to 60°C. After reacting for 4 hours, transfer the system to dichloromethane, wash the system with 20 mL of saturated brine, dry with anhydrous magnesium sulfate, and remove the solvent by evaporation under reduced pressure to obtain modified vegetable oil;

[0096] A3, adding 9 mg of microcrystalline wax to the modified vegetable oil in step A2, raising the temperature to 80°C and stirring at 30 rpm for 15 minutes, and then leaving the gel at 20°C for 24 hours to obtain grease 6;

[0097] Wherein, the bio-based adhesive is prepared by the following steps:

[0098] B1, add 0.585g 0.1mol / L 2-morpholineethanesulfonic acid solution and 0.0876g 0.05mol / L NaCl solution to 30mL sterile deionized water, adjust the pH value of the system to 5.1 with NaOH solution, and obtain 2-morpholineethanesulfonic acid buffer for standby use;

[0099] B2. Take 30 mL of the 2-morpholineethanesulfonic acid buffer prepared in step B1, add 3 g of carboxymethyl cellulose, 0.192 g of EDC, 0.115 g of N-hydroxysuccinimide and 0.5 g of dopamine hydrochloride, stir well for 12 hours at room temperature and nitrogen atmosphere, then freeze-dry in a freeze dryer, and then resuspend in 30 mL of deionized water to obtain a bio-based adhesive.

[0100] Comparative Example 2: A high-performance powder metallurgy oil-containing bearing, comprising an inner ring 3, an outer ring 5, a steel ball 1, a retainer 2 and a dust cover 4, with grease 6 between the inner ring 3 and the outer ring 5, and the grease 6 is sealed by the dust cover 4.

[0101] A method for manufacturing a high-performance powder metallurgy oil-containing bearing comprises the following steps:

[0102] S1, adding iron powder into the inner ring 3 and the outer ring 5 pressing mold to press into blanks, the pressure during the pressing process is 300Mpa, the pressing time is 5 minutes, and the blanks are obtained respectively;

[0103] S2. The blank obtained in step S1 is subjected to vacuum sintering: the vacuum degree is set to 1.3×10 -3 Pa, raising the temperature in the furnace to 200°C for pre-sintering for 10 minutes; then raising the temperature to 700°C at a heating rate of 10°C / min, treating for 20 minutes, and naturally cooling to room temperature to obtain a sintered blank;

[0104] S3, demould and remove the sintered blank, wash the surface of the inner ring 3 and the outer ring 5 with anhydrous ethanol respectively, then install the dust cover 4, inject 5wt% sulfuric acid solution into the sealed cavity formed by the inner ring 3, the outer ring 5 and the dust cover 4, fill it up and treat it for 10 minutes, then remove the dust cover 4 and rinse the sealed cavity with anhydrous ethanol, then wash it with clean water, dry it and place it in a vacuum oil immersion machine for vacuum oil immersion, and the vacuum degree is 1.5×10 -3 pa, the oil temperature is 40°C, and an inner ring 3 and an outer ring 5 are obtained; then the inner ring 3, the outer ring 5, the steel ball 1 and the retainer 2 are assembled, 20 mL of bio-based adhesive is injected between the inner ring 3 and the outer ring 5, and 50 mL of grease 6 is injected after the coating is complete, and then a dust cover 4 is used for sealing, so as to obtain a high-performance powder metallurgy oil-containing bearing;

[0105] Wherein, lubricating grease 6 is prepared by following steps:

[0106] A1. Weigh 300 mg of vegetable oil, 100 mg of dodecane and 8 mL of freshly prepared 0.5 mol / L sodium hydroxide methanol solution and stir them at room temperature until they are uniform. Then, raise the system temperature to 80° C., add 7 mL of boron trifluoride methanol solution after treating for 0.5 hour, raise the temperature to 100° C., treat for 10 minutes, then continue to add 5 mL of n-heptane, treat for 3 minutes, wash the system with 20 mL of saturated sodium chloride solution, let stand for stratification, and retain the upper liquid to obtain esterified vegetable oil;

[0107] A2. Add 50 mg of ethanolamine to the esterified vegetable oil obtained in step A1, stir at room temperature for 5 minutes, add 0.45 ml of 0.05 mol / L sodium methoxide solution and raise the system temperature to 60°C. After reacting for 4 hours, transfer the system to dichloromethane, wash the system with 20 mL of saturated brine, dry with anhydrous magnesium sulfate, and remove the solvent by evaporation under reduced pressure to obtain modified vegetable oil;

[0108] A3, adding 9 mg of microcrystalline wax to the modified vegetable oil in step A2, raising the temperature to 80°C and stirring at 30 rpm for 15 minutes, and then leaving the gel at 20°C for 24 hours to obtain grease 6;

[0109] Wherein, the bio-based adhesive is prepared by the following steps:

[0110] B1, add 0.585g 0.1mol / L 2-morpholineethanesulfonic acid solution and 0.0876g 0.05mol / L NaCl solution to 30mL sterile deionized water, adjust the pH value of the system to 5.1 with NaOH solution, and obtain 2-morpholineethanesulfonic acid buffer for standby use;

[0111] B2. Take 30 mL of the 2-morpholineethanesulfonic acid buffer prepared in step B1, add 3 g of carboxymethyl cellulose, 0.192 g of EDC, 0.115 g of N-hydroxysuccinimide and 0.5 g of dopamine hydrochloride, stir well for 12 hours at room temperature and nitrogen atmosphere, then freeze-dry in a freeze dryer, and then resuspend in 30 mL of deionized water to obtain a bio-based adhesive.

[0112] Comparative Example 3: A high-performance powder metallurgy oil-containing bearing, comprising an inner ring 3, an outer ring 5, a steel ball 1, a retainer 2 and a dust cover 4, with grease 6 between the inner ring 3 and the outer ring 5, and the grease 6 is sealed by the dust cover 4.

[0113] A method for manufacturing a high-performance powder metallurgy oil-containing bearing comprises the following steps:

[0114] S1. Mix B4C, V2O5 and SiO2 in a mass ratio of 1:1:2 to obtain a reinforced powder, wherein the particle size of B4C and V2O5 is 0-50 μm, and the particle size of SiO2 is 0-20 nm;

[0115] Then, the iron powder and the reinforcing powder were placed in a mixer and stirred at a rate of 15 rpm for 20 minutes to obtain a base powder, wherein the amount of the reinforcing powder used was 1 wt % of the iron powder;

[0116] S2, then add the base powder into the inner ring 3 and the outer ring 5 pressing molds to press into blanks, the pressure during the pressing process is 300 MPa, the pressing time is 5 minutes, and the primary blanks are obtained respectively;

[0117] S3, vacuum sintering the blank obtained in step S2: setting the vacuum degree to 1.3×10 -3 Pa, raising the temperature in the furnace to 200°C for pre-sintering for 10 minutes; then raising the temperature to 700°C at a heating rate of 10°C / min, treating for 20 minutes, and naturally cooling to room temperature to obtain a sintered blank;

[0118] S4, demould the sintered blank, wash the surface of the inner ring 3 and the outer ring 5 with anhydrous ethanol, then install the dust cover 4, inject 5wt% sulfuric acid solution into the sealed cavity formed by the inner ring 3, the outer ring 5 and the dust cover 4, fill it up and treat it for 10 minutes, then remove the dust cover 4 and rinse the sealed cavity with anhydrous ethanol, then wash it with clean water, dry it, and place it in a vacuum oil immersion machine for vacuum oil immersion, and the vacuum degree is 1.5×10 -3 pa, the oil temperature is 40°C, and an inner ring 3 and an outer ring 5 are obtained; then the inner ring 3, the outer ring 5, the steel ball 1 and the retainer 2 are assembled, 70 mL of grease 6 is injected between the inner ring 3 and the outer ring 5, and then a dust cover 4 is used for sealing, thereby obtaining a high-performance powder metallurgy oil-containing bearing;

[0119] Wherein, lubricating grease 6 is prepared by following steps:

[0120] A1. Weigh 300 mg of vegetable oil, 100 mg of dodecane and 8 mL of freshly prepared 0.5 mol / L sodium hydroxide methanol solution and stir them at room temperature until they are uniform. Then, raise the system temperature to 80° C., add 7 mL of boron trifluoride methanol solution after treating for 0.5 hour, raise the temperature to 100° C., treat for 10 minutes, then continue to add 5 mL of n-heptane, treat for 3 minutes, wash the system with 20 mL of saturated sodium chloride solution, let stand for stratification, and retain the upper liquid to obtain esterified vegetable oil;

[0121] A2. Add 50 mg of ethanolamine to the esterified vegetable oil obtained in step A1, stir at room temperature for 5 minutes, add 0.45 ml of 0.05 mol / L and treat for 3-5 minutes and raise the system temperature to 60°C. After reacting for 4 hours, transfer the system to dichloromethane, wash the system with 20 mL of saturated brine and dry with anhydrous magnesium sulfate, evaporate under reduced pressure to remove the solvent, and obtain modified vegetable oil;

[0122] A3, adding 9 mg of microcrystalline wax to the modified vegetable oil in step A2, raising the temperature to 80°C and stirring at 30 rpm for 15 minutes, and then leaving the gel at 20°C for 24 hours to obtain grease 6;

[0123] Comparative Example 4: A high-performance powder metallurgy oil-containing bearing, comprising an inner ring 3, an outer ring 5, a steel ball 1, a retainer 2 and a dust cover 4, with grease 6 between the inner ring 3 and the outer ring 5, and the grease 6 is sealed by the dust cover 4.

[0124] A method for manufacturing a high-performance powder metallurgy oil-containing bearing comprises the following steps:

[0125] S1. Mix B4C, V2O5 and SiO2 in a mass ratio of 1:1:2 to obtain a reinforced powder, wherein the particle size of B4C and V2O5 is 0-50 μm, and the particle size of SiO2 is 0-20 nm;

[0126] Then, the iron powder and the reinforcing powder were placed in a mixer and stirred at a rate of 15 rpm for 20 minutes to obtain a base powder, wherein the amount of the reinforcing powder used was 1 wt % of the iron powder;

[0127] S2, then add the base powder into the inner ring 3 and the outer ring 5 pressing molds to press into blanks, the pressure during the pressing process is 300 MPa, the pressing time is 5 minutes, and the primary blanks are obtained respectively;

[0128] S3, vacuum sintering the blank obtained in step S2: setting the vacuum degree to 1.3×10 -3 Pa, raising the temperature in the furnace to 200°C for pre-sintering for 10 minutes; then raising the temperature to 700°C at a heating rate of 10°C / min, treating for 20 minutes, and naturally cooling to room temperature to obtain a sintered blank;

[0129] S4, demould the sintered blank, wash the surface of the inner ring 3 and the outer ring 5 with anhydrous ethanol, then install the dust cover 4, inject 5wt% sulfuric acid solution into the sealed cavity formed by the inner ring 3, the outer ring 5 and the dust cover 4, fill it up and treat it for 10 minutes, then remove the dust cover 4 and rinse the sealed cavity with anhydrous ethanol, then wash it with clean water, dry it, and place it in a vacuum oil immersion machine for vacuum oil immersion, and the vacuum degree is 1.5×10 -3pa, the oil temperature is 40°C, and an inner ring 3 and an outer ring 5 are obtained; then the inner ring 3, the outer ring 5, the steel ball 1 and the retainer 2 are assembled, 20 mL of bio-based adhesive is injected between the inner ring 3 and the outer ring 5, and 50 mL of grease 6 is injected after the coating is complete, and then a dust cover 4 is used for sealing, so as to obtain a high-performance powder metallurgy oil-containing bearing;

[0130] Wherein, lubricating grease 6 is prepared by following steps:

[0131] 9 mg of microcrystalline wax was added to 300 mg of vegetable oil, the temperature was raised to 80° C., and then stirred at 30 rpm for 15 minutes, and then allowed to stand at 20° C. for 24 hours to form a gel, thereby obtaining grease 6;

[0132] Wherein, the bio-based adhesive is prepared by the following steps:

[0133] B1, add 0.585g 0.1mol / L 2-morpholineethanesulfonic acid solution and 0.0876g 0.05mol / L NaCl solution to 30mL sterile deionized water, adjust the pH value of the system to 5.1 with NaOH solution, and obtain 2-morpholineethanesulfonic acid buffer for standby use;

[0134] B2. Take 30 mL of the 2-morpholineethanesulfonic acid buffer prepared in step B1, add 3 g of carboxymethyl cellulose, 0.192 g of EDC, 0.115 g of N-hydroxysuccinimide and 0.5 g of dopamine hydrochloride, stir well for 12 hours at room temperature and nitrogen atmosphere, then freeze-dry in a freeze dryer, and then resuspend in 30 mL of deionized water to obtain a bio-based adhesive.

[0135] The performance of the oil-containing bearings prepared in Examples 1-3 and Comparative Examples 1-4 was tested. The basic rated dynamic load, basic rated static load and limiting speed of the oil-containing bearings prepared in different groups were tested. The test results are shown in Table 1 below.

[0136] Table 1 Performance test of oil-containing bearings prepared in Examples 1-3 and Comparative Examples 1-4

[0137] Group Basic dynamic load rating (kN) Basic static load rating (kN) Limit speed (r / min) Example 1 60.3 38.9 5000 Example 2 63.6 41.0 5300 Example 3 62.1 40.1 5100 Comparative Example 1 56.3 37.4 4800 Comparative Example 2 52.1 34.7 4600 Comparative Example 3 49.2 31.6 4200 Comparative Example 4 50.1 32.0 4000

[0138] As can be seen from the results in Table 1, the oil-containing bearing prepared in Example 2 exhibits the best performance, with the highest dynamic and static loads and limiting speed. As can be seen from the results in Comparative Examples 1 and 3, pickling the inner ring 3 and the outer ring 5 of the bearing and using a layer of adhesive can improve the stability of the bearing during operation, so that it can exhibit a greater load and speed. As can be seen from the results in Comparative Example 2, using components such as nano-SiO2 and boron carbide to enhance the iron powder can effectively improve the overall mass transfer effect of the bearing, faster heat dissipation and faster grease penetration efficiency during operation, and better improve its working performance such as load and speed. As can be seen from the results in Comparative Example 4, modifying the vegetable oil can improve the compatibility of the vegetable oil with the adhesive, improve the balance of the pores inside the inner ring 3 and the outer ring 5 of the bearing, and improve the mass transfer of the grease 6 therein.

[0139] The oil-containing bearings prepared in Examples 1-3 and Comparative Examples 1-4 are now tested for grease leakage resistance. According to the method described in GB / T32321-2015, the oil-containing bearings prepared in different groups are tested, and the test results are shown in Table 2 below.

[0140] Table 2 Grease leakage prevention performance test of oil-containing bearings prepared in Examples 1-3 and Comparative Examples 1-4

[0141] Group Fat leakage rate (%) Example 1 0.22 Example 2 0.10 Example 3 0.29 Comparative Example 1 0.34 Comparative Example 2 0.30 Comparative Example 3 1.36 Comparative Example 4 1.01

[0142] From the results in Table 2, it can be seen that the oil-containing bearing prepared in Example 2 has the best grease 6 retention effect. From the results in Comparative Examples 1 and 3, it can be seen that the bio-based adhesive can improve the stability of the grease 6, and pickling the inner ring 3 and the outer ring 5 of the bearing can improve the effect of the bio-based adhesive. From the results in Comparative Example 2, it can be seen that adding reinforcing materials to the matrix of the inner ring 3 and the outer ring 5 can also improve the stability of the grease 6. From the results in Comparative Example 4, it can be seen that improving the compatibility of the grease 6 and the bio-based adhesive is also conducive to reducing the seepage of grease on the bearing.

[0143] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0144] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A method for manufacturing a high-performance powder metallurgy oil-containing bearing, It is characterized in that The following steps are involved: S1, placing iron powder and reinforcing powder in a mixer and stirring to obtain base powder, wherein the amount of reinforcing powder used is 1-3wt% of the iron powder; S2, then adding the base powder into the inner ring and outer ring pressing molds to press into blanks, the pressure during the pressing process is 300-450Mpa, the pressing time is 5-20 minutes, and the primary blanks are obtained respectively; S3, vacuum sintering the blank obtained in step S2: setting the vacuum degree to 1.3×10 -3 Pa, raising the temperature in the furnace to 200-300°C for pre-sintering for 10-15 minutes; then raising the temperature to 700-750°C at a heating rate of 10-20°C / min, treating for 20-30 minutes, and then naturally cooling to room temperature to obtain a sintered blank; S4, demoulding the sintered blank, treating the outer surface of the inner ring and the inner surface of the outer ring with acid, then washing with clean water, drying and placing in a vacuum oil immersion machine for vacuum oil immersion, the vacuum degree is 1.5×10 -3 -3×10 -3 pa, the oil temperature is 40-80°C, and the inner ring and the outer ring are obtained; then the inner ring, the outer ring, the steel ball and the retainer are assembled, and the bio-based adhesive is injected between the inner ring and the outer ring. After the coating is complete, grease is injected, and then a dust cover is used for sealing, so as to obtain a high-performance powder metallurgy oil-containing bearing; Wherein, the lubricating grease is prepared by the following steps: A1. Stir vegetable oil, dodecane and sodium hydroxide methanol solution at room temperature until uniform, then raise the system temperature to 80°C, add boron trifluoride methanol solution after treating for 0.5-2 hours, raise the temperature to 80-120°C, treat for 10-30 minutes, then add n-heptane for 3-5 minutes, wash the system, stand and separate, and retain the upper liquid to obtain esterified vegetable oil; A2, adding ethanolamine to the esterified vegetable oil obtained in step A1, stirring at room temperature for 5-10 minutes, adding sodium methoxide solution for 3-5 minutes and raising the system temperature to 50-70°C, reacting for 4-5 hours, transferring the system to dichloromethane, washing the system and drying to obtain modified vegetable oil; A3, adding microcrystalline wax to the modified vegetable oil in step A2, raising the temperature to 80-100°C, stirring at 30-60 rpm for 15-30 minutes, and then standing at 20°C for 24 hours to gel, thereby obtaining lubricating grease; Wherein, the bio-based adhesive is prepared by the following steps: B1, adding 2-morpholineethanesulfonic acid solution and NaCl solution into sterile deionized water, adjusting the pH value of the system to 5.1, and obtaining 2-morpholineethanesulfonic acid buffer for standby use; B2. Dissolve carboxymethyl cellulose, EDC, N-hydroxysuccinimide and dopamine hydrochloride in 2-morpholineethanesulfonic acid buffer, stir well for 12-48 hours at room temperature under an inert gas atmosphere, then freeze-dry in a freeze dryer, and then resuspend in deionized water to obtain a bio-based adhesive.

2. According to the method for manufacturing a high-performance powder metallurgy oil-containing bearing as described in claim 1, It is characterized in that The mass ratio of vegetable oil, ethanolamine and microcrystalline wax is 300:(50-100):(9-80).

3. According to the method for manufacturing a high-performance powder metallurgy oil-containing bearing as described in claim 1, It is characterized in that In step B2, the mass ratio of carboxymethyl cellulose to dopamine hydrochloride is (3-6):(0.5-1.5).

4. According to the method for manufacturing a high-performance powder metallurgy oil-containing bearing as described in claim 1, It is characterized in that In step S4, the specific operation of the acid treatment is: Wash the surface of the inner ring and outer ring with anhydrous ethanol respectively, then install the dust cover, inject the acid into the sealed cavity formed by the inner ring, outer ring and dust cover, and treat it for 10-30 minutes after filling, then remove the dust cover and rinse the sealed cavity with anhydrous ethanol.

5. The method for manufacturing a high performance powder metallurgy oil-containing bearing according to claim 4, It is characterized in that The acid solution is a 5-10wt% sulfuric acid solution.

6. The method for manufacturing a high performance powder metallurgy oil-containing bearing according to claim 1, It is characterized in that In step S4, the steel ball is at least one of carbon steel, chrome steel ball, and stainless steel ball, and the material of the dust cover is at least one of fluorinated rubber, polytetrafluoroethylene, ethylene propylene rubber, fluorosilicone rubber, polyurethane, and chloroprene rubber.

7. The method for manufacturing a high performance powder metallurgy oil-containing bearing according to claim 1, It is characterized in that In step S1, the reinforced powder is composed of B 4 C.V 2 O 5 and SiO 2 The mixture is obtained by mixing according to the mass ratio of (1-2):(1-2):(2-4), wherein B 4 C.V 2 O 5 The particle size is 0-50μm, SiO 2 The particle size is 0-20nm.

8. A bearing made by the method for making a high-performance powder metallurgy oil-containing bearing as claimed in any one of claims 1 to 7, It is characterized in that The utility model comprises an inner ring, an outer ring, steel balls, a retainer and a dust cover. There is grease between the inner ring and the outer ring, and the grease is sealed by the dust cover.

Citation Information

Patent Citations

  • High-performance iron-based powder metallurgy oil-containing self-lubricating bearing and production process thereof

    CN102062149A

  • Bearing ring and roller bearing having said bearing ring

    CN106460932A

  • Preparation method of conductive adhesive hydrogel

    CN112442194A

  • Biodegradable lubricating grease and preparation method thereof

    CN112662454A

  • Rolling bearing

    CN1357693A