Waterproof and shock-absorbing polyurethane elastomer for intelligent water meter potting and preparation method thereof

By using perfluoroalkanoyl chloride modified polyether polyol and diisocyanate system, the problems of existing materials being easily damaged and insufficient hydrophobic in low temperature environments are solved, and good waterproofing, anti-freeze and shock relief are achieved Performance, extends service life and simplifies the preparation process.

CN118530430BActive Publication Date: 2024-11-12SHANDONG INOV POLYURETHANE
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411000501.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

The existing smart water meter potting materials are prone to damage in low temperature environments and lack good waterproof, anti-freeze and shock cushioning properties. The common materials lack hydrophobicity and resilience, resulting in insufficient sealing effect and service life.

Method used

Using the waterproof and cushioned polyurethane elastomer for intelligent water meter potting prepared from hydrophobic modified polyether polyol and diisocyanate systems, the surface energy of the molecular chain segment is reduced by perfluoroalkanoyl chloride modified polyether polyol, and the hydrophobicity and resilience are improved. , and ensure the aging resistance and shock cushioning effect of the material through specific component proportions and process flow.

Benefits of technology

It realizes the good hydrophobicity, resilience and aging resistance of smart water meter potting materials, extends the service life of the product, avoids the risk of using volatile highly toxic chemicals, and simplifies the preparation process.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the technical field of polyurethane elastomers, and specifically to a waterproof and shock-absorbing polyurethane elastomer for smart water meter potting and a preparation method thereof. The preparation method of the waterproof and shock-absorbing polyurethane elastomer for smart water meter potting is composed of a component A and a component B with a mass ratio of 1: (0.95-1.05), wherein the component A includes a hydrophobically modified polyether polyol, an antioxidant, and a catalyst, and the component B includes a hydrophobically modified polyether polyol and a diisocyanate; the hydrophobically modified polyether polyol is a polyether polyol modified with perfluoroalkanoyl chloride; the functionality of the polyether polyol is 3 and the number average molecular weight is 300-5000. The present invention introduces a perfluoroalkyl chain into the molecular chain of the polyether polyol, reduces the surface energy of the molecular chain segment of the polyurethane elastomer, improves the hydrophobicity of the polyurethane elastomer as a potting material, and greatly improves its waterproof and shock-absorbing properties and aging resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyurethane elastomers, and in particular to a waterproof and shock-absorbing polyurethane elastomer for potting of smart water meters and a preparation method thereof. Background Art

[0002] Smart water meter is a new type of water meter that uses modern microelectronics technology, modern sensor technology, and smart IC card technology to measure water consumption and transmit data and settle transactions. The application environment of smart water meters is complex and diverse, especially in the northern region where the temperature is low in winter. In order to prevent the LCD screen and circuit board of the smart water meter from being damaged by low temperature, the product needs to be moisture-proof, waterproof, and antifreeze, which puts higher requirements on the potting materials of smart water meters. In addition, strong collisions and impacts can also cause damage to smart water meters. Therefore, the potting materials used for smart water meters also need to have good shock-absorbing effects.

[0003] At present, there are three common smart water meter potting materials on the market: epoxy resin, silicone, and polyurethane. The advantages of epoxy resin potting glue are good adhesion to hard materials, good high temperature resistance and electrical insulation; however, after curing, the colloid is relatively hard and brittle, which can easily damage electronic components, and has weak resistance to cold and hot changes. It is easy to crack after being subjected to cold and hot shocks, which will cause water vapor to penetrate into the electronic components through the cracks. Polyurethane potting glue has excellent low temperature resistance and shock absorption performance, a wide range of colloid hardness adjustment, good elongation and tear resistance, good adhesion to common substrate materials, high adhesion, and good wear resistance; the disadvantages are poor high temperature resistance, poor aging resistance, and easy discoloration of the colloid. The advantages of silicone potting glue are strong anti-aging ability, good weather resistance and good impact resistance; however, compared with epoxy resin potting glue and polyurethane potting glue, its mechanical properties such as tensile strength and shear strength are poor, the hardness adjustment range is narrow, the bonding performance with the substrate is slightly poor, and the water absorption rate is high, which makes its sealing effect poor.

[0004] Regarding polyurethane potting glue, patent CN111286004A discloses a hydrophobic polyurethane anti-condensation airtight plugging material, wherein the component A is diisocyanate and polyisocyanate, and the component B is modified polyester polyol, polyolefin polyol, catalyst, auxiliary agent, and filler. The hydrophobicity and thermal hydrolysis resistance of the polyurethane plugging material are improved by compounding modified polyester polyol and polyolefin polyol, and compounding diisocyanate and polyisocyanate. However, the toluene diisocyanate used in the invention belongs to a high environmental risk product, and the product obtained by the polyol and isocyanate system used in the invention has poor resilience, resulting in poor shock absorbing effect of the product.

[0005] Patent CN116217880A discloses a polyurethane rubber for ceramic piston sealing, which uses alkyl chloride to modify high-functionality polyester polyols to prepare low-surface-energy polyester polyols with long alkyl chains as side chains, which not only improves the hydrophobicity and temperature resistance of the product, reduces endogenous heat, but also solves the difficulty of high viscosity and difficult operation of polyester / MDI type prepolymer components. However, the water contact angle of the polyurethane elastomer prepared by the method is low, and the hydrophobic effect is average. Summary of the invention

[0006] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a waterproof and shock-absorbing polyurethane elastomer for smart water meter potting, which has good hydrophobicity, resilience and aging resistance, gives the product good waterproof and shock-absorbing effects, and extends the service life of the product. The present invention also provides a preparation method thereof.

[0007] The waterproof and shock-absorbing polyurethane elastomer for potting of the smart water meter of the present invention is composed of component A and component B in a mass ratio of 1: (0.95-1.05), wherein component A includes the following raw materials in parts by mass:

[0008] 98-98.8 parts of hydrophobically modified polyether polyol,

[0009] Antioxidant 0.9-1.5 parts,

[0010] Catalyst 0.3-0.5 parts;

[0011] The B component includes the following raw materials in parts by weight:

[0012] 47-59 parts of hydrophobically modified polyether polyol;

[0013] 41-53 parts of diisocyanate;

[0014] The hydrophobically modified polyether polyol is a polyether polyol modified by perfluoroalkanoyl chloride; the functionality of the polyether polyol is 3 and the number average molecular weight is 300-5000; the general structural formula of the perfluoroalkanoyl chloride is CF 3 -(CF 2 ) n -CO-Cl, n is an integer between 2 and 6.

[0015] Preferably, the polyether polyols used in the hydrophobically modified polyether polyols of component A and component B include polyether polyols with a functionality of 3 and a number average molecular weight of 300-500 and polyether polyols with a functionality of 3 and a number average molecular weight of 3000-5000.

[0016] Preferably, the polyether polyol is one or more of C304, MN3050D, and 330NG, all of which are produced by Shandong Bluestar Dongda Chemical Co., Ltd.

[0017] Preferably, the perfluoroalkanoyl chloride is one or more of perfluorobutyryl chloride, perfluorohexanoyl chloride and perfluorooctanoyl chloride.

[0018] The preparation method of the hydrophobically modified polyether polyol is as follows: dissolving a polyether polyol having a moisture content of less than 0.05wt.% in tetrahydrofuran, adding an acid-binding agent triethylamine, heating to 60-70°C, adding perfluoroalkanoyl chloride dropwise while stirring under a constant temperature condition, and completing the addition within 0.5-2h, wherein the molar ratio of the polyether polyol to the perfluoroalkanoyl chloride is 1:(0.95-1.05), maintaining the reaction temperature at 60-70°C, reacting at a constant temperature for 5-6h, filtering to remove triethylamine hydrochloride, washing the residue with ethanol first, then with deionized water, and drying to obtain the hydrophobically modified polyether polyol.

[0019] The antioxidant is one or more of UV-44, UV-21, UV-02, UV-01, 1039, and 1076, all of which are produced by Shanghai BASF Chemical Co., Ltd.

[0020] The catalyst is one or more of CUCAT-E01, CUCAT-E02, and CUCAT-E05, all of which are produced by Guangzhou Yourun Synthetic Materials Co., Ltd.

[0021] The diisocyanate is one or more of isophorone diisocyanate (IPDI), 4,4-dicyclohexylmethane diisocyanate (HMDI), and hexamethylene diisocyanate (HDI).

[0022] The method for preparing the waterproof and shock-absorbing polyurethane elastomer for intelligent water meter potting of the present invention comprises the following steps:

[0023] (1) Component B: Under nitrogen protection, add hydrophobically modified polyether polyol to diisocyanate, raise the temperature to 95-100°C, keep the temperature for 3-4 hours, vacuum degas, and cool down to obtain component B;

[0024] (2) Component A: Under nitrogen protection, the hydrophobically modified polyether polyol, catalyst and antioxidant are mixed, the temperature is raised to 95-100°C, and vacuum dehydration is performed until the moisture content is less than 0.05wt.%, thereby obtaining component A;

[0025] (3) When in use, mix components A and B in a mass ratio of 1: (0.95-1.05) and cast them into a smart water meter. Vulcanize at room temperature to obtain a waterproof and shock-absorbing polyurethane elastomer for smart water meter encapsulation.

[0026] In step (3), during casting, the temperature of the mixture of components A and B is maintained at 25-35°C, and the operating time of casting is 20-30 minutes.

[0027] In step (3), the room temperature vulcanization time is not less than 7 days.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] (1) The present invention uses perfluoroalkanoyl chloride to modify polyether polyol, introduces perfluoroalkyl chains into the polyether polyol molecular chain, reduces the surface energy of the polyurethane elastomer molecular chain segment, and improves the hydrophobicity and aging resistance of the polyurethane elastomer as a potting material; at the same time, the present invention uses polyether polyols with different molecular weights for modification, improves the resilience of the polyurethane elastomer, and enhances its shock-absorbing effect;

[0030] (2) The hydrophobically modified polyether polyol and aliphatic isocyanate system used in the present invention does not contain volatile highly toxic chemicals and has little impact on the health of operators;

[0031] (3) The preparation method of the present invention is simple and easy to implement, and the viscosity of the prepolymer component is moderate, which is convenient for subsequent pouring by a pouring machine. DETAILED DESCRIPTION

[0032] The present invention is further described below with reference to the examples. The raw materials used in the examples, unless otherwise specified, are all commercially available conventional raw materials; the process methods used in the examples, unless otherwise specified, are all conventional methods in the art.

[0033] Some of the raw materials used in the examples are described as follows:

[0034] C304: polyether polyol, 3 functionalities, molecular weight 375, Shandong Bluestar Dongda Chemical Co., Ltd.;

[0035] MN3050D: polyether polyol, 3 functionalities, molecular weight 3000, Shandong Bluestar Dongda Chemical Co., Ltd.;

[0036] 330NG: polyether polyol, 3 functional groups, molecular weight 5000, Shandong Bluestar Dongda Chemical Co., Ltd.;

[0037] PE-304: polyester polyol, 3 functional groups, molecular weight 375, Shandong Yinuowei Polyurethane Co., Ltd.;

[0038] HMDI: 4,4-dicyclohexylmethane diisocyanate, 2-functionality, Wanhua Chemical Group Co., Ltd.

[0039] IPDI: isophorone diisocyanate, Wanhua Chemical Group Co., Ltd.;

[0040] HDI: Hexamethylene diisocyanate, Wanhua Chemical Group Co., Ltd.;

[0041] MDI-50: diphenylmethane diisocyanate, Wanhua Chemical Group Co., Ltd.;

[0042] CD-C: carbodiimide modified MDI, Covestro Polymers (China) Co., Ltd.;

[0043] MI: diphenyl diisocyanate, Shanghai BASF Chemical Co., Ltd.;

[0044] UV-44, UV-21, UV-01, UV-02, 1076, 1039: antioxidants, Shanghai BASF Chemical Co., Ltd.;

[0045] CUCAT-E01, CUCAT-E02, CUCAT-E05: Catalysts, Guangzhou Yourun Synthetic Materials Co., Ltd.

[0046] The hydrophobically modified polyether polyols used in the examples and comparative examples were prepared by the following method:

[0047] (1) Hydrophobically modified polyether polyol C304-04:

[0048] Dissolve polyether polyol C304 with a moisture content of less than 0.05wt.% in tetrahydrofuran, add acid binding agent triethylamine, raise the temperature to 60°C, add perfluorobutyryl chloride dropwise while stirring under constant temperature conditions, and complete the addition within 1 hour, wherein the molar ratio of polyether polyol C304 to perfluorobutyryl chloride is 1:0.95, maintain the reaction temperature at 60°C, react at constant temperature for 5 hours, filter to remove triethylamine hydrochloride, wash the residue with ethanol first, then with deionized water, and dry to obtain hydrophobically modified polyether polyol C304-04.

[0049] (2) Hydrophobically modified polyether polyol MN3050D-06:

[0050] The polyether polyol MN3050D with a moisture content of less than 0.05wt.% was dissolved in tetrahydrofuran, and triethylamine, an acid binding agent, was added. The temperature was raised to 65°C, and perfluorohexanoyl chloride was added dropwise with stirring under constant temperature conditions. The addition was completed within 0.5h, wherein the molar ratio of polyether polyol MN3050D and perfluorohexanoyl chloride was 1:1. The reaction temperature was maintained at 65°C and the reaction was carried out at a constant temperature for 6h. The triethylamine hydrochloride was removed by filtration, and the residue was washed with ethanol first and then with deionized water. After drying, the hydrophobically modified polyether polyol MN3050D-06 was obtained.

[0051] (3) Hydrophobically modified polyether polyol 330N-08:

[0052] Dissolve polyether polyol 330N with a moisture content of less than 0.05wt.% in tetrahydrofuran, add acid binding agent triethylamine, raise the temperature to 70°C, add perfluorooctanoyl chloride dropwise while stirring under constant temperature conditions, and complete the addition within 2 hours, wherein the molar ratio of polyether polyol 330N to perfluorooctanoyl chloride is 1:1.05, maintain the reaction temperature at 70°C, react at constant temperature for 6 hours, filter to remove triethylamine hydrochloride, wash the residue with ethanol first, then with deionized water, and dry to obtain hydrophobically modified polyether polyol 330N-08.

[0053] (4) Hydrophobically modified polyester polyol PE-304-04:

[0054] PE-304 with a moisture content of less than 0.05wt.% is dissolved in tetrahydrofuran, and triethylamine, an acid binding agent, is added. The temperature is raised to 65°C, and perfluorobutyryl chloride is added dropwise while stirring under constant temperature conditions. The addition is completed within 2 hours, wherein the molar ratio of polyester polyol PE-304 to perfluorobutyryl chloride is 1:1. The reaction temperature is maintained at 65°C, and the reaction is carried out at a constant temperature for 6 hours. The triethylamine hydrochloride is filtered out, and the residue is first washed with ethanol and then with deionized water. After drying, the hydrophobically modified polyester polyol PE-304-04 is obtained.

[0055] Example 1

[0056] A method for preparing a waterproof and shock-absorbing polyurethane elastomer for potting of a smart water meter comprises the following steps:

[0057] (1) Component B: By weight, under nitrogen protection, add 47 parts of hydrophobically modified polyether polyol C304-04 to 53 parts of IPDI, raise the temperature to 95°C, keep the temperature for 4 hours, evacuate to -0.01 MPa for degassing for 1 hour, and cool down to obtain a prepolymer with an isocyanate content of 12.8 wt.%, which is used as component B;

[0058] (2) Component A: In parts by mass, under nitrogen protection, 83 parts of hydrophobically modified polyether polyol C304-04, 15.8 parts of hydrophobically modified polyether polyol MN3050-06, 0.3 parts of catalyst CUCAT-E01, 0.3 parts of antioxidant UV-44, 0.3 parts of antioxidant UV-01, and 0.3 parts of antioxidant 1076 were mixed, the temperature was raised to 95°C, and the mixture was vacuumed to -0.01 MPa for dehydration until the moisture content was less than 0.05 wt.%, thereby obtaining component A;

[0059] (3) When in use, mix components A and B evenly in a mass ratio of 1:1.05, maintain the temperature of the mixture of components A and B at 25°C, and the operable time for casting is 30 minutes. Within the operable time, cast the mixture of components A and B into the smart water meter, and then vulcanize it at room temperature for 7 days to obtain the waterproof and shock-absorbing polyurethane elastomer for smart water meter encapsulation.

[0060] Example 2

[0061] A method for preparing a waterproof and shock-absorbing polyurethane elastomer for potting of a smart water meter comprises the following steps:

[0062] (1) Component B: by weight, under nitrogen protection, add 51 parts of hydrophobically modified polyether polyol 330N-08 to 49 parts of HMDI, raise the temperature to 100°C, keep the temperature for 3 hours, evacuate to -0.01 MPa for degassing for 1 hour, and cool down to obtain a prepolymer with an isocyanate content of 14.9 wt.%, which is used as component B;

[0063] (2) Component A: In parts by mass, under nitrogen protection, 98.1 parts of hydrophobically modified polyether polyol C304-04, 0.3 parts of catalyst CUCAT-E01, 0.2 parts of catalyst CUCAT-E02, 0.5 parts of antioxidant UV-21, 0.5 parts of antioxidant UV-02, and 0.4 parts of antioxidant 1039 were mixed, the temperature was raised to 100°C, and the pressure was evacuated to -0.01 MPa for dehydration until the moisture content was less than 0.05 wt.%, thereby obtaining component A;

[0064] (3) When in use, mix components A and B evenly in a mass ratio of 1:1.05, maintain the temperature of the mixture of components A and B at 35°C, and the operable time for casting is 20 minutes. Within the operable time, cast the mixture of components A and B into the smart water meter, and then vulcanize it at room temperature for 7 days to obtain the waterproof and shock-absorbing polyurethane elastomer for smart water meter encapsulation.

[0065] Example 3

[0066] A method for preparing a waterproof and shock-absorbing polyurethane elastomer for potting of a smart water meter comprises the following steps:

[0067] (1) Component B: by weight, under nitrogen protection, add 59 parts of hydrophobically modified polyether polyol MN3050-06 to 20 parts of IPDI and 21 parts of HMDI, raise the temperature to 100°C, keep the temperature for 3.5 hours, evacuate to -0.01 MPa for degassing for 1 hour, and cool down to obtain a prepolymer with an isocyanate content of 12.8 wt.%, which is used as component B;

[0068] (2) Component A: In parts by mass, under nitrogen protection, mix 83 parts of hydrophobically modified polyether polyol C304-04, 15 parts of hydrophobically modified polyether polyol 330N-08, 0.5 parts of catalyst CUCAT-E05, 0.5 parts of antioxidant UV-21, 0.5 parts of antioxidant UV-02, and 0.5 parts of antioxidant 1039, raise the temperature to 95°C, evacuate to -0.01 MPa and dehydrate until the moisture content is less than 0.05 wt.%, thereby obtaining component A;

[0069] (3) When in use, mix components A and B evenly in a mass ratio of 1:0.95, maintain the temperature of the mixture of components A and B at 30°C, and the operable time for casting is 24 minutes. Within the operable time, cast the mixture of components A and B into the smart water meter, and then vulcanize it at room temperature for 7 days to obtain the waterproof and shock-absorbing polyurethane elastomer for smart water meter encapsulation.

[0070] Example 4

[0071] A method for preparing a waterproof and shock-absorbing polyurethane elastomer for potting of a smart water meter comprises the following steps:

[0072] (1) Component B: By weight, add 10 parts of hydrophobically modified polyether polyol C304-04 and 45 parts of hydrophobically modified polyether polyol 330N-08 to 20 parts of IPDI and 25 parts of HMDI under nitrogen protection, raise the temperature to 95°C, keep the temperature for 4 hours, evacuate to -0.01 MPa for degassing for 1 hour, and cool down to obtain a prepolymer with an isocyanate content of 13.4 wt.%, which is used as component B;

[0073] (2) Component A: In parts by mass, under nitrogen protection, 85 parts of hydrophobically modified polyether polyol C304-04, 13 parts of hydrophobically modified polyether polyol MN3050-06, 0.5 parts of catalyst CUCAT-E01, 0.5 parts of antioxidant UV-44, and 0.5 parts of antioxidant 1076 were mixed, heated to 100°C, and vacuumed to -0.01 MPa for dehydration until the moisture content was less than 0.05 wt.%, thereby obtaining component A;

[0074] (3) When in use, mix components A and B in a mass ratio of 1:1, maintain the temperature of the mixture of components A and B between 30°C, and the operable time for casting is 24 minutes. Cast the mixture of components A and B into the smart water meter within the operable time, and then vulcanize at room temperature for 7 days to obtain the waterproof and shock-absorbing polyurethane elastomer for smart water meter encapsulation.

[0075] Comparative Example 1

[0076] The only difference between this comparative example and Example 1 is that the hydrophobically modified polyether polyol C304-04 and the hydrophobically modified polyether polyol MN3050-06 in component A are replaced by equal parts by weight of polyether polyol C304 and polyether polyol MN3050, respectively.

[0077] Comparative Example 2

[0078] The only difference between this comparative example and Example 4 is that the hydrophobically modified polyether polyol C304-04 and the hydrophobically modified polyether polyol 330N-08 in component B are replaced by equal parts by mass of polyether polyol C304 and polyether polyol 330N, respectively.

[0079] Comparative Example 3

[0080] The A and B components of this comparative example both use unmodified polyether polyols, and the preparation method is as follows:

[0081] (1) Component B: by weight, under nitrogen protection, add 45 parts of polyether polyol MN3050 to 25 parts of CD-C and 30 parts of MI, raise the temperature to 85°C, keep the temperature for 4 hours, evacuate to -0.01 MPa for degassing for 1 hour, and cool down to obtain a prepolymer with an isocyanate content of 15.5 wt.%, which is used as component B;

[0082] (2) Component A: In parts by mass, under nitrogen protection, mix 37 parts of polyether polyol C304, 61 parts of polyether polyol MN3050, 0.5 parts of catalyst CUCAT-E01, 0.5 parts of antioxidant UV-44, 0.5 parts of antioxidant UV01, and 0.5 parts of antioxidant 1076, raise the temperature to 100°C, evacuate to -0.01 MPa and dehydrate until the moisture content is less than 0.05 wt.%, thereby obtaining component A;

[0083] (3) When in use, mix components A and B in a mass ratio of 1:1, keep the temperature of the mixture of components A and B at 25°C, and the operation time for casting is 30 minutes.

[0084] The polyurethane elastomer for smart water meter potting is obtained by casting and then vulcanizing at room temperature for 7 days.

[0085] Comparative Example 4

[0086] Commercially available silicone potting glue is used for smart water meter potting, model is Kasu K6100.

[0087] Comparative Example 5

[0088] Component A of this comparative example uses hydrophobically modified polyester polyol PE-304-04, and the preparation method is as follows:

[0089] (1) Component B: By weight, under nitrogen protection, add 47 parts of hydrophobically modified polyether polyol C304-04 to 53 parts of IPDI, raise the temperature to 95°C, keep the temperature for 4 hours, evacuate to -0.01 MPa for degassing for 1 hour, and cool down to obtain a prepolymer with an isocyanate content of 12.8 wt.%, which is used as component B;

[0090] (2) Component A: In parts by mass, under nitrogen protection, mix 99.1 parts of hydrophobically modified polyester polyol PE-304-04, 0.3 parts of catalyst CUCAT-E01, 0.3 parts of antioxidant UV-44, and 0.3 parts of antioxidant 1076, raise the temperature to 95°C, evacuate to -0.01 MPa and dehydrate until the moisture content is less than 0.05 wt.%, to obtain component A;

[0091] (3) When in use, mix components A and B evenly in a mass ratio of 1:1.15, maintain the temperature of the mixture of components A and B at 25°C, and the operable time for casting is 30 minutes. Within the operable time, cast the mixture of components A and B into the smart water meter, and then vulcanize it at room temperature for 7 days to obtain the polyurethane elastomer for smart water meter potting.

[0092] The performance tests were conducted on the smart water meter potting materials (polyurethane elastomer or silicone potting glue) of each embodiment and comparative example, wherein the 25°C hardness was tested in accordance with the standard (GB / T531-1999); the rebound rate was tested in accordance with the standard (GB / T1681-2009); the water contact angle was tested in accordance with the standard GB / T 30693-2014; the water absorption test was the mass change rate after the double 85 test (GB / T10586-2006), and the calculation formula was = (after the test - before the test) / before the test × 100%. The test results are shown in Table 1.

[0093] Table 1 Product performance test results of various embodiments and comparative examples

[0094] Test items 25℃ Hardness / A Rebound rate / % Water absorption / % Water contact angle / ° Example 1 62 36 0.04 130 Example 2 64 43 0.03 143 Example 3 57 41 0.038 134 Example 4 59 38 0.035 138 Comparative Example 1 67 45 0.06 106 Comparative Example 2 65 48 0.05 120 Comparative Example 3 70 49 0.1 67 Comparative Example 4 15 20 0.5 75 Comparative Example 5 70 25 0.14 128

[0095] It can be seen from Table 1 that:

[0096] Compared with Example 1, the A component of Comparative Example 1 uses common polyether polyol, which has high surface energy, and the prepared polyurethane elastomer has poor hydrophobic effect.

[0097] Compared with Example 4, the B component of Comparative Example 2 uses ordinary polyether polyol, which has a high surface energy. However, because the A component uses hydrophobically modified polyether polyol, the proportion of hydrophobic segments is high, so the hydrophobic effect of the prepared polyurethane elastomer is slightly better than that of Comparative Example 1.

[0098] Compared with Examples 1-4, the A and B components of Comparative Example 3 both use common polyether polyols, which have a higher surface energy, resulting in the worst hydrophobic effect of the polyurethane elastomer prepared therefrom.

[0099] Compared with Examples 1-4, the silicone potting adhesive of Comparative Example 4 not only has poor hydrophobicity, but also has a hardness and elasticity far lower than the polyurethane elastomer of the present invention.

[0100] Compared with Example 1, hydrophobically modified polyester polyol is used in component A of Comparative Example 5. Since the polyester polyol has extremely strong crystallinity, the ester bonds on the molecular chain segments have strong rigidity and poor flexibility, the polyurethane elastomer prepared therefrom has high hardness, but poor resilience and poor shock-absorbing effect.

[0101] The polyurethane elastomer prepared in Example 2 has the best hydrophobic effect. This is because the hydrophobic modifier chain segment used in Example 2 is the longest, so the polyurethane elastomer prepared therefrom has the best hydrophobic effect, the best hydrolysis resistance, and the lowest water absorption rate.

Claims

1. A waterproof and shock-absorbing polyurethane elastomer for smart water meter potting, characterized in that: It is composed of component A and component B in a mass ratio of 1: (0.95-1.05), wherein component A includes the following raw materials in mass fractions: 98-98.8 parts of hydrophobically modified polyether polyol, Antioxidant 0.9-1.5 parts, Catalyst 0.3-0.5 parts; The B component includes the following raw materials in parts by weight: 47-59 parts of hydrophobically modified polyether polyol; 41-53 parts of diisocyanate; The hydrophobically modified polyether polyol is a polyether polyol modified with perfluoroalkanoyl chloride; the functionality of the polyether polyol is 3 and the number average molecular weight is 300-5000; the general structural formula of the perfluoroalkanoyl chloride is CF3-(CF2) n -CO-Cl, n is an integer between 2 and 6.

2. The waterproof and shock-absorbing polyurethane elastomer for intelligent water meter potting according to claim 1 is characterized in that: The perfluoroalkanoyl chloride is one or more of perfluorobutyryl chloride, perfluorohexanoyl chloride and perfluorooctanoyl chloride.

3. The waterproof and shock-absorbing polyurethane elastomer for intelligent water meter potting according to claim 1 is characterized in that: The preparation method of the hydrophobically modified polyether polyol is as follows: dissolving a polyether polyol having a moisture content of less than 0.05wt.% in tetrahydrofuran, adding an acid-binding agent triethylamine, heating to 60-70°C, adding perfluoroalkanoyl chloride dropwise while stirring under a constant temperature condition, and completing the addition within 0.5-2h, wherein the molar ratio of the polyether polyol to the perfluoroalkanoyl chloride is 1:(0.95-1.05), maintaining the reaction temperature at 60-70°C, reacting at a constant temperature for 5-6h, filtering to remove triethylamine hydrochloride, washing the residue with ethanol first, then with deionized water, and drying to obtain the hydrophobically modified polyether polyol.

4. The waterproof and shock-absorbing polyurethane elastomer for intelligent water meter potting according to claim 1 is characterized in that: The antioxidant is one or more of UV-44, UV-21, UV-02, UV-01, 1039, and 1076.

5. The waterproof and shock-absorbing polyurethane elastomer for intelligent water meter potting according to claim 1 is characterized in that: The catalyst is one or more of CUCAT-E01, CUCAT-E02, and CUCAT-E05.

6. The waterproof and shock-absorbing polyurethane elastomer for intelligent water meter potting according to claim 1 is characterized in that: The diisocyanate is one or more of isophorone diisocyanate, 4,4-dicyclohexylmethane diisocyanate and hexamethylene diisocyanate.

7. A method for preparing the waterproof and shock-absorbing polyurethane elastomer for smart water meter potting according to any one of claims 1 to 6, characterized in that: The following steps are involved: (1) Component B: Under nitrogen protection, add hydrophobically modified polyether polyol to diisocyanate, raise the temperature to 95-100°C, keep the temperature for 3-4 hours, vacuum degas, and cool down to obtain component B; (2) Component A: Under nitrogen protection, the hydrophobically modified polyether polyol, catalyst and antioxidant are mixed, the temperature is raised to 95-100°C, and vacuum dehydration is performed until the moisture content is less than 0.05wt.%, thereby obtaining component A; (3) When in use, mix components A and B in a mass ratio of 1: (0.95-1.05) and cast them into a smart water meter. Vulcanize at room temperature to obtain a waterproof and shock-absorbing polyurethane elastomer for encapsulating smart water meters.

8. The method for preparing the waterproof and shock-absorbing polyurethane elastomer for intelligent water meter potting according to claim 7, characterized in that: In step (3), during casting, the temperature of the mixture of components A and B is maintained at 25-35°C, and the operating time of casting is 20-30 minutes.

9. The method for preparing the waterproof and shock-absorbing polyurethane elastomer for intelligent water meter potting according to claim 7, characterized in that: In step (3), the room temperature vulcanization time is not less than 7 days.

Citation Information

Patent Citations

  • Hydrophobic polyurethane anti-condensation airtight plugging material and preparation method thereof

    CN111286004A

  • Polyurethane rubber for sealing ceramic piston and preparation method thereof

    CN116217880A

  • Microporous polyurethane elastomer composition with excellent dynamic performance and method for preparing same