A high-strength, high-creep-resistance, thermally conductive nylon composite material and preparation method thereof

By adding polycarbonate and thermal filler to nylon materials and using supercritical carbon dioxide to assist processing, the problem of insufficient impact and creep resistance of existing nylon materials has been solved, significantly improving the performance of composite materials and suitable for industrial production.

CN118530582BActive Publication Date: 2024-11-08赤途实业(上海)有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411009428.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-08
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

The impact strength and creep resistance of existing nylon materials cannot meet market demand, limiting their application scope.

Method used

The ratio of 60 parts of nylon, 30-50 parts of polycarbonate, 10-15 parts of thermal filler, 2-3 parts of antioxidant, 3-4 parts of silane coupling agent, and 2-3 parts of lubricant is adopted to pass the supercritical The preparation method of carbon dioxide injection improves the compatibility and flowability of materials, improves impact strength and creep resistance.

Benefits of technology

It significantly improves the impact strength and creep resistance of the composite material, solves the layering phenomenon of polycarbonate and nylon, enhances the flowability and dispersion of the melt, reduces the processing temperature, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118530582B_ABST
    Figure CN118530582B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of polymer materials, and in particular to a high-strength, high-creep-resistant, heat-conducting nylon composite material and a preparation method thereof. The raw materials for its preparation, in terms of weight, include 60 parts of nylon, 30-50 parts of polycarbonate, 10-15 parts of heat-conducting filler, 2-3 parts of antioxidant, 3-4 parts of silane coupling agent, and 2-3 parts of lubricant; the mass ratio of the nylon to the polycarbonate is 6:(3-5); the silane coupling agent includes one or more of trimethoxy (3-methoxypropyl) silane, vinyl tri-tert-butyl peroxy silane, and γ-(methacryloyloxy) propyl trimethoxy silane; the lubricant includes one or more of tributyl phosphate, pentaerythritol stearate, and glycerol tristearate; the preparation method of the high-strength, high-creep-resistant, heat-conducting nylon composite material includes a step of injecting supercritical carbon dioxide. The present invention enhances the creep performance and impact performance of the composite material and has a wide range of application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a high-strength, high-creep resistance, and thermally conductive nylon composite material and a preparation method thereof. Background Art

[0002] Nylon, as a common thermoplastic, is widely used because of its good comprehensive properties, including heat resistance, wear resistance, low friction coefficient, good corrosion resistance, and certain flame retardancy. With the rapid development of the nylon material industry, the performance requirements for materials are getting higher and higher. At present, the impact strength and creep resistance of nylon materials in the existing market are increasingly unable to meet the market demand, limiting its application scope.

[0003] Prior art CN101717568B discloses a polycarbonate / nylon 6 alloy material and a preparation method thereof. The impact and temperature resistance of the alloy material vary with the ratio of PC / PA6, and the alloy material has stable tensile and bending properties. However, the creep resistance of the alloy material still cannot meet the market demand. Therefore, the development of a high-strength, high-creep resistance, and thermally conductive nylon composite material has important application value. Summary of the invention

[0004] In order to solve the problems in the prior art, the first aspect of the present invention provides a high-strength, high-creep-resistant, thermally conductive nylon composite material, wherein the raw materials for its preparation, in terms of weight parts, include 60 parts of nylon, 30-50 parts of polycarbonate, 10-15 parts of thermally conductive filler, 2-3 parts of antioxidant, 3-4 parts of silane coupling agent, and 2-3 parts of lubricant; the mass ratio of the nylon to the polycarbonate is 6:(3-5); the silane coupling agent includes one or more of trimethoxy (3-methoxypropyl) silane, vinyl tri-tert-butyl peroxy silane, and γ-(methacryloyloxy)propyl trimethoxy silane; the lubricant includes one or more of tributyl phosphate, pentaerythritol stearate, and glycerol tristearate;

[0005] The method for preparing the high-strength, high-creep resistance and thermally conductive nylon composite material comprises the step of injecting supercritical carbon dioxide.

[0006] Furthermore, the raw materials for preparing the high-strength, high-creep resistance and thermally conductive nylon composite material include, by weight, 60 parts of nylon, 40 parts of polycarbonate, 15 parts of thermally conductive filler, 3 parts of antioxidant, 4 parts of silane coupling agent and 3 parts of lubricant.

[0007] Preferably, the nylon includes one or more of nylon 6, nylon 66, nylon 1010, and nylon 12.

[0008] Furthermore, the nylon is nylon 6.

[0009] Preferably, the polycarbonate comprises bisphenol A polycarbonate.

[0010] Preferably, the thermally conductive filler includes one or more of nano-boron nitride, nano-aluminum oxide, and graphite.

[0011] Furthermore, the thermally conductive filler is graphite.

[0012] Preferably, the antioxidant includes one or more of hindered amine antioxidants, phosphite antioxidants, and hindered phenol antioxidants.

[0013] Furthermore, the antioxidant is a composite antioxidant of a phosphite antioxidant and a hindered phenol antioxidant.

[0014] Furthermore, the phosphite antioxidant is antioxidant 168; and the hindered phenol antioxidant is antioxidant 1010.

[0015] Preferably, the silane coupling agent includes one or more of trimethoxy (3-methoxypropyl) silane, vinyl tri-tert-butyl peroxy silane, and γ-(methacryloyloxy)propyl trimethoxy silane.

[0016] Furthermore, the silane coupling agent is trimethoxy (3-methoxypropyl) silane.

[0017] In the art, the solubility parameters of polycarbonate and nylon are quite different, and the two are thermodynamically incompatible. When polycarbonate and nylon are blended, stratification will occur significantly, and amino exchange reactions are likely to occur, resulting in a decrease in the molecular weight of the two, thereby affecting the performance of the composite material. This application study found that adding a silane coupling agent to the system can effectively solve the incompatibility phenomenon when polycarbonate and nylon are blended, especially when the silane coupling agent is trimethoxy (3-methoxypropyl) silane, the compatibility of polycarbonate and nylon can be significantly improved.

[0018] Preferably, the lubricant includes one or more of tributyl phosphate, pentaerythritol stearate, and glyceryl tristearate.

[0019] Furthermore, the lubricant is tributyl phosphate.

[0020] The present application has found that the addition of nylon, polycarbonate, and thermally conductive fillers to the system will cause the fluidity of the melt to deteriorate during processing. The present application has found that the addition of a lubricant to the system can significantly increase the fluidity of the melt, while also improving the impact strength and creep resistance of the prepared composite material. In particular, the performance is particularly outstanding when the lubricant is tributyl phosphate.

[0021] The second aspect of the present invention provides a method for preparing a high-strength, high-creep-resistance, thermally conductive nylon composite material, which specifically comprises the following steps:

[0022] S1: Put nylon, polycarbonate, thermal conductive filler, antioxidant, silane coupling agent and lubricant into a mixer and mix for 3-5 minutes to obtain a mixture.

[0023] S2: The mixture is added from the feeding port of a twin-screw extruder, supercritical carbon dioxide is injected into the twin-screw extruder, and a high-strength, high-creep-resistance, and thermally conductive nylon composite material is obtained through extrusion and granulation.

[0024] Preferably, in step S1, the mixer speed is 100 rpm and the mixing time is 5 min.

[0025] Preferably, the temperature of the twin-screw extruder in S2 is set as follows: the temperature of the first zone is 200-210°C, the temperature of the second zone is 210-230°C, the temperature of the third zone is 220-240°C, the temperature of the fourth zone is 230-240°C, the temperature of the fifth zone is 220-230°C, the temperature of the sixth zone is 210-220°C, and the temperature of the seventh zone is 200-210°C; in S2, supercritical carbon dioxide is injected into at least one of the fifth and sixth zones.

[0026] Furthermore, supercritical carbon dioxide is injected into the fifth zone in S2.

[0027] Furthermore, the injection amount of the supercritical carbon dioxide is 6-9L.

[0028] Furthermore, the supercritical carbon dioxide is injected at a temperature of 60° C. and a pressure of 90 atm.

[0029] The present application study found that the addition of supercritical carbon dioxide can reduce the temperature of the processing process and promote the dispersion and fluidity of the mixture. At the same time, the addition of supercritical carbon dioxide can also increase the compatibility of polycarbonate and nylon components and improve the impact strength and creep resistance of the composite material.

[0030] Beneficial Effects

[0031] 1. The composite material prepared by the present invention contains polycarbonate, which can improve the impact resistance and creep resistance of nylon.

[0032] 2. The composite material prepared by the present invention uses a specific silane coupling agent trimethoxy (3-methoxypropyl) silane, which can effectively solve the delamination phenomenon caused by the mixing of polycarbonate and nylon, and significantly improve the compatibility of polycarbonate and nylon.

[0033] 3. The composite material prepared by the present invention uses a specific lubricant, tributyl phosphate, which can significantly increase the melt dispersibility and fluidity, and at the same time improve the impact strength and creep resistance of the prepared composite material.

[0034] 4. The present invention adopts a specific preparation process, and supercritical carbon dioxide is added during the processing, which can not only promote melt dispersion and fluidity, but also increase the compatibility of polycarbonate and nylon components, and improve the impact strength and creep resistance of the composite material.

[0035] 5. The raw materials of the high-strength, high-creep-resistance and thermally conductive nylon composite material of the present invention are easily available, easy to prepare, low in cost, and easy to industrially produce. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 The creep performance diagram of the composite materials prepared in Examples 1-3 and Comparative Examples 1-3. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the examples and drawings. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. The experimental methods for which specific conditions are not specified in the examples are carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used that do not specify the manufacturer are all conventional products that can be purchased commercially.

[0038] Example 1

[0039] The first aspect of the present embodiment provides a high-strength, high-creep-resistance, thermally conductive nylon composite material, the raw materials for its preparation, in parts by weight, include 60 parts of nylon, 30 parts of polycarbonate, 10 parts of thermally conductive filler, 2 parts of antioxidant, 3 parts of silane coupling agent, and 2 parts of lubricant.

[0040] The nylon is nylon 6.

[0041] The polycarbonate is bisphenol A type polycarbonate.

[0042] The thermally conductive filler is graphite.

[0043] The antioxidant is a composite antioxidant of antioxidant 168 and antioxidant 1010.

[0044] The mass ratio of the antioxidant 168 to the antioxidant 1010 is 1:1.

[0045] The silane coupling agent is trimethoxy (3-methoxypropyl) silane.

[0046] The lubricant is tributyl phosphate.

[0047] A second aspect of the present embodiment provides a method for preparing a high-strength, high-creep resistance, and thermally conductive nylon composite material, comprising the following steps:

[0048] S1: Put nylon, polycarbonate, thermal conductive filler, antioxidant, silane coupling agent and lubricant into a mixer and mix them for 5 minutes at a speed of 100 rpm to obtain a mixture.

[0049] S2: Add the mixture from the feeding port of the twin-screw extruder. The temperature of the first zone of the twin-screw extruder is 200°C, the temperature of the second zone is 210°C, the temperature of the third zone is 220°C, the temperature of the fourth zone is 230°C, the temperature of the fifth zone is 220°C, the temperature of the sixth zone is 220°C, and the temperature of the seventh zone is 200°C. At the same time, supercritical carbon dioxide is injected into the fifth zone. The injection amount of supercritical carbon dioxide is 6L, and the temperature of supercritical carbon dioxide injection is 60°C and the pressure is 90atm. After extrusion and granulation, a high-strength, high-creep-resistant and thermally conductive nylon composite material is obtained.

[0050] The supercritical carbon dioxide injection amount is 6% of the mass of the mixture obtained in S1.

[0051] Example 2

[0052] This embodiment is basically the same as Embodiment 1, except that:

[0053] The high-strength, high-creep-resistance, and thermally conductive nylon composite material is prepared from raw materials, by weight, including 60 parts of nylon, 40 parts of polycarbonate, 15 parts of thermally conductive filler, 3 parts of antioxidant, 4 parts of silane coupling agent, and 3 parts of lubricant.

[0054] A second aspect of the present embodiment provides a method for preparing a high-strength, high-creep resistance, and thermally conductive nylon composite material, comprising the following steps:

[0055] S1: Put nylon, polycarbonate, thermal conductive filler, antioxidant, silane coupling agent and lubricant into a mixer and mix them for 5 minutes at a speed of 100 rpm to obtain a mixture.

[0056] S2: Add the mixture from the feeding port of the twin-screw extruder, the temperature of the first zone of the twin-screw extruder is 210℃, the temperature of the second zone is 220℃, the temperature of the third zone is 230℃, the temperature of the fourth zone is 230℃, the temperature of the fifth zone is 220℃, the temperature of the sixth zone is 210℃, and the temperature of the seventh zone is 210℃. At the same time, supercritical carbon dioxide is injected into the fifth zone, the injection amount of supercritical carbon dioxide is 9L, the temperature of supercritical carbon dioxide injection is 60℃, and the pressure is 90atm. After extrusion and granulation, a high-strength, high-creep-resistant and thermally conductive nylon composite material is obtained.

[0057] The supercritical carbon dioxide injection amount is 5.1% of the mass of the mixture obtained in S1.

[0058] Example 3

[0059] This embodiment is basically the same as Embodiment 2, except that:

[0060] The raw materials for preparing the high-strength, high-creep-resistance and thermally conductive nylon composite material include, by weight, 60 parts of nylon, 50 parts of polycarbonate, 15 parts of thermally conductive filler, 3 parts of antioxidant, 4 parts of silane coupling agent and 3 parts of lubricant.

[0061] A second aspect of the present embodiment provides a method for preparing a high-strength, high-creep resistance, and thermally conductive nylon composite material, comprising the following steps:

[0062] S1: Put nylon, polycarbonate, thermal conductive filler, antioxidant, silane coupling agent and lubricant into a mixer and mix them for 5 minutes at a speed of 100 rpm to obtain a mixture.

[0063] S2: Add the mixture from the feeding port of the twin-screw extruder. The temperature of the first zone of the twin-screw extruder is 210°C, the temperature of the second zone is 230°C, the temperature of the third zone is 240°C, the temperature of the fourth zone is 240°C, the temperature of the fifth zone is 230°C, the temperature of the sixth zone is 220°C, and the temperature of the seventh zone is 210°C. At the same time, supercritical carbon dioxide is injected into the fifth zone. The injection amount of supercritical carbon dioxide is 9L, and the temperature of supercritical carbon dioxide injection is 60°C and the pressure is 90atm. After extrusion and granulation, a high-strength, high-creep-resistant and thermally conductive nylon composite material is obtained.

[0064] The supercritical carbon dioxide injection amount is 4.8% of the mass of the mixture obtained in S1.

[0065] Comparative Example 1

[0066] This comparative example is basically the same as Example 1, except that:

[0067] The first aspect of the present comparative example provides a high-strength, high-creep-resistance, thermally conductive nylon composite material, the raw materials for its preparation, in parts by weight, include 60 parts of nylon, 30 parts of polycarbonate, 10 parts of thermally conductive filler, 2 parts of antioxidant, and 3 parts of silane coupling agent.

[0068] A second aspect of the present embodiment provides a method for preparing a high-strength, high-creep resistance, and thermally conductive nylon composite material, comprising the following steps:

[0069] S1: Put nylon, polycarbonate, thermal conductive filler, antioxidant and silane coupling agent into a mixer and mix them for 5 minutes at a speed of 100 rpm to obtain a mixture.

[0070] S2: Add the mixture from the feeding port of the twin-screw extruder. The temperature of the first zone of the twin-screw extruder is 200°C, the temperature of the second zone is 210°C, the temperature of the third zone is 220°C, the temperature of the fourth zone is 230°C, the temperature of the fifth zone is 220°C, the temperature of the sixth zone is 220°C, and the temperature of the seventh zone is 200°C. At the same time, supercritical carbon dioxide is injected into the fifth zone. The injection amount of supercritical carbon dioxide is 6L, and the temperature of supercritical carbon dioxide injection is 60°C and the pressure is 90atm. After extrusion and granulation, a high-strength, high-creep-resistant and thermally conductive nylon composite material is obtained.

[0071] The supercritical carbon dioxide injection amount is 4% of the mass of the mixture obtained in S1.

[0072] Comparative Example 2

[0073] This comparative example is basically the same as Example 2, except that:

[0074] The high-strength, high-creep-resistance, and thermally conductive nylon composite material is prepared from raw materials, by weight, including 60 parts of nylon, 40 parts of polycarbonate, 15 parts of thermally conductive filler, 3 parts of antioxidant, 4 parts of silane coupling agent, and 3 parts of lubricant.

[0075] A second aspect of the present embodiment provides a method for preparing a high-strength, high-creep resistance, and thermally conductive nylon composite material, comprising the following steps:

[0076] S1: Put nylon, polycarbonate, thermal conductive filler, antioxidant and silane coupling agent into a mixer and mix them for 5 minutes at a speed of 100 rpm to obtain a mixture.

[0077] S2: Add the mixture from the feeding port of the twin-screw extruder, the temperature of the first zone of the twin-screw extruder is 210°C, the temperature of the second zone is 220°C, the temperature of the third zone is 230°C, the temperature of the fourth zone is 230°C, the temperature of the fifth zone is 220°C, the temperature of the sixth zone is 210°C, and the temperature of the seventh zone is 210°C. After extrusion and granulation, a high-strength, high-creep-resistant and thermally conductive nylon composite material is obtained.

[0078] Comparative Example 3

[0079] This comparative example is basically the same as Example 1, except that:

[0080] The first aspect of the present comparative example provides a high-strength, high-creep-resistance, thermally conductive nylon composite material, the raw materials for its preparation, in parts by weight, include 100 parts of nylon, 10 parts of thermally conductive filler, 3 parts of antioxidant, 4 parts of silane coupling agent, and 3 parts of lubricant.

[0081] A second aspect of the present embodiment provides a method for preparing a high-strength, high-creep resistance, and thermally conductive nylon composite material, comprising the following steps:

[0082] S1: Put nylon, thermal conductive filler, antioxidant and silane coupling agent into a mixer and mix them for 5 minutes at a speed of 100 rpm to obtain a mixture.

[0083] S2: Add the mixture from the feeding port of the twin-screw extruder. The temperature of the first zone of the twin-screw extruder is 210°C, the temperature of the second zone is 230°C, the temperature of the third zone is 240°C, the temperature of the fourth zone is 240°C, the temperature of the fifth zone is 230°C, the temperature of the sixth zone is 220°C, and the temperature of the seventh zone is 210°C. At the same time, supercritical carbon dioxide is injected into the fifth zone. The injection amount of supercritical carbon dioxide is 6L, and the temperature of supercritical carbon dioxide injection is 60°C and the pressure is 90atm. After extrusion and granulation, a high-strength, high-creep-resistant and thermally conductive nylon composite material is obtained.

[0084] The supercritical carbon dioxide injection amount is 3.6% of the mass of the mixture obtained in S1.

[0085] Performance Testing

[0086] 1. Izod beam notched impact strength: tested in accordance with GB / T1843-2008 standard.

[0087] 2. Thermal conductivity: longitudinal test according to ISO 22007-2.

[0088] 3. Creep performance: The test was conducted using a dynamic thermal analyzer (DMAQ800) in a tensile mode with a load of 0.2 MPa and a test time of 30 min.

[0089] The composite materials prepared in Examples 1-3 of the present invention and Comparative Examples 1-3 were subjected to the above performance tests. The results are shown in Tables 1 and Figure 1 .

[0090] Table 1

[0091]

[0092] According to the test results, the present invention increases the creep and impact properties of the composite material by adding polycarbonate to the nylon 6 matrix and improving the fluidity of the melt with the assistance of supercritical carbon dioxide and tributyl phosphate, wherein Example 2 is the best example.

[0093] It can be seen from the data in Table 1 that in Example 2 of the present invention and Comparative Example 1, when supercritical carbon dioxide is injected, the fluidity of the melt is poor due to the lack of tributyl phosphate, resulting in uneven dispersion of the components, and the impact strength of the composite material finally prepared is low; from the experimental results of Comparative Example 2, it can be concluded that when supercritical carbon dioxide is not injected, part of the tributyl phosphate decomposes during the melt processing due to the high processing temperature, which ultimately affects the impact strength of the composite material; from the experimental results of Comparative Example 3, it can be concluded that when supercritical carbon dioxide is injected, the impact strength of the prepared composite material is very low due to the lack of polycarbonate components.

[0094] from Figure 1 It can be seen from the data curves in that, in Example 2 of the present invention and Comparative Example 1, when supercritical carbon dioxide is injected, the fluidity of the melt is poor due to the lack of butyl triphosphate, resulting in uneven dispersion of the components, and the creep performance of the composite material finally prepared is low; from the experimental results of Comparative Example 2, it can be concluded that when supercritical carbon dioxide is not injected, the bonding ability between the components decreases during the melt processing, which ultimately affects the creep performance of the composite material; from the experimental results of Comparative Example 3, it can be concluded that when supercritical carbon dioxide is injected, the creep performance of the prepared composite material is very low due to the lack of polycarbonate component.

[0095] The above experimental results show that the high-strength, high-creep-resistance, and thermally conductive nylon composite materials prepared in Examples 1-3 of the present invention have excellent impact strength and creep properties, as well as certain thermal conductivity, compared with Comparative Example 3.

[0096] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present invention. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. It is particularly pointed out that for those skilled in the art, any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention should be included in the scope of protection of the present invention.

Claims

1. A high-strength, high-creep-resistance, thermally conductive nylon composite material, characterized in that: The raw materials for its preparation, by weight, include 60 parts of nylon, 40 parts of polycarbonate, 15 parts of thermal conductive filler, 3 parts of antioxidant, 4 parts of silane coupling agent, and 3 parts of lubricant; The mass ratio of nylon to polycarbonate is 6:4; the silane coupling agent is trimethoxy (3-methoxypropyl) silane; the lubricant is tributyl phosphate; the antioxidant is a composite antioxidant of antioxidant 168 and antioxidant 1010, and the mass ratio of antioxidant 168 to antioxidant 1010 is 1:1; The nylon is nylon 6; the polycarbonate is bisphenol A polycarbonate; and the thermal conductive filler is graphite; The preparation method of the high-strength, high-creep-resistance, thermally conductive nylon composite material specifically comprises the following steps: S1: putting nylon, polycarbonate, thermal conductive filler, antioxidant, silane coupling agent and lubricant into a mixer and mixing for 5 minutes at a speed of 100 rpm to obtain a mixture; S2: adding the mixture from the feeding port of the twin-screw extruder, the temperature of the first zone of the twin-screw extruder is 210°C, the temperature of the second zone is 220°C, the temperature of the third zone is 230°C, the temperature of the fourth zone is 230°C, the temperature of the fifth zone is 220°C, the temperature of the sixth zone is 210°C, and the temperature of the seventh zone is 210°C. At the same time, supercritical carbon dioxide is injected into the fifth zone, the injection amount of supercritical carbon dioxide is 9L, the temperature of supercritical carbon dioxide injection is 60°C, and the pressure is 90atm; after extrusion and granulation, a high-strength, high-creep-resistant and thermally conductive nylon composite material is obtained; The supercritical carbon dioxide injection amount is 5.1% of the mass of the mixture obtained in S1.