A kind of fracturing fluid containing silicon rubber and preparation method thereof
By using ingredients such as silicone rubber, sulfonic acid-modified maleopimarium amides, and hydroxy-quaternary ammonium-modified maleopimarium amides in the fracturing fluid, the problem of poor performance of existing fracturing fluids at high temperatures has been solved and achieved High-efficiency shear performance and oil recovery efficiency under high temperature and high pressure conditions.
Patent Information
- Application Number
- CN202410992966.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-24
AI Technical Summary
Existing fracturing fluids have poor performance in high-temperature environments, making it difficult to maintain efficient shear performance and affecting oil recovery efficiency.
Silicone-containing rubber fracturing fluid is used. Its composition includes silicone rubber, sulfonic acid-modified maleopimarium amate, hydroxy-quaternary ammonium-modified maleopimarium and sodium salicylate. It is prepared through a specific synthesis method to form a high-viscosity and shear-resistant fracturing fluids.
The temperature and shear resistance of the fracturing fluid is significantly improved in high-temperature environments, ensuring that it can still maintain high oil recovery efficiency under high-temperature and high-pressure conditions.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of oil and gas field development, in particular to a silicone rubber-containing fracturing fluid and a preparation method thereof. Background Art
[0002] Fracturing fluid is a common oil and gas production increase technology, the purpose of which is to press cracks into the oil and gas layers to increase production. Existing fracturing fluids include oil-based fracturing fluids, alcohol-based fracturing fluids, water-based fracturing fluids, etc. During use, fracturing fluids must have high shear resistance, high viscosity, high temperature resistance and other properties. If the performance does not meet the requirements, it will affect its oil recovery efficiency. For example, application number CN201510269729.3 discloses a low-temperature resistant fracturing fluid for oil production and its preparation method. The invented fracturing fluid has excellent low-temperature resistance, good sand carrying capacity at low temperatures, and good shear performance; however, its high-temperature resistance effect has not been improved. Summary of the invention
[0003] 1. Technical issues to be resolved
[0004] In view of the deficiencies in the prior art, the present invention provides a silicone rubber-containing fracturing fluid and a preparation method thereof, which has good high temperature resistance and shear resistance effects.
[0005] (II) Technical solution
[0006] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a silicone rubber-containing fracturing fluid and a preparation method thereof, a silicone rubber-containing fracturing fluid, comprising the following components by weight: 5-7 parts by weight of silicone rubber, 6-10 parts by weight of sulfonic acid-modified maleopimaric acid ester, 4-6 parts by weight of hydroxyl-quaternary ammonium-modified maleopimaric acid ester, 0.4-0.8 parts by weight of sodium salicylate, and 20-30 parts by weight of water.
[0007] Preferably, the preparation method of the sulfonic acid modified maleopimaric acid ester is:
[0008] (1) Maleic anhydride and pimaric acid were added to the reactor, heated in an oil bath at 120-140°C for 18-25 min, and then p-tolyl urea was added under stirring. After the addition, the reaction was continued for 3-4 h. After the reaction was completed, the reaction was cooled to room temperature and recrystallized from methanol for 2-3 times to obtain intermediate 1;
[0009] (2) Add intermediate 1 and 1,3-bis(dimethylamino)-2-propanol to N,N-dimethylformamide solvent, stir to dissolve, continue to add p-toluenesulfonic acid catalyst, react at 90-110°C for 8-12h, distill under reduced pressure after reaction, filter and dry to obtain intermediate 2;
[0010] (3) Under a nitrogen atmosphere, add intermediate 2 and 1,3-propane sultone into a reactor, stir and mix, and react at 20-25° C. for 20-30 h. After reaction, filter, wash and dry to obtain sulfonic acid-modified maleopimaric acid ester.
[0011] Preferably, the mass ratio of maleic anhydride, pimaric acid and p-tolyl urea in (1) is 1:0.4-0.6.
[0012] Preferably, in the (2), the mass ratio of the intermediate 1, 1,3-bis(dimethylamino)-2-propanol, and p-toluenesulfonic acid catalyst is 1.3-1.5:1:0.01-0.03.
[0013] Preferably, the mass ratio of the intermediate 2 to 1,3-propane sultone in (3) is 1:1.4-1.8.
[0014] Preferably, the preparation method of the hydroxy-quaternary ammonium modified maleopimaronamide is:
[0015] S1. 5-8 parts by weight of intermediate 1 is added to 10-15 parts by weight of thionyl chloride, dispersed evenly, reacted at 70-80 ° C for 20-24h, filtered after the reaction, washed and dried to obtain an acyl chloride intermediate 1;
[0016] S2. Add 8-14 parts by weight of the acyl chloride intermediate 1 and 6-15 parts by weight of diethanolamine to N,N-dimethylformamide solvent, stir to dissolve, continue to add 1-2 parts by weight of pyridine catalyst, react at 75-90 ° C for 8-14h, and then distill under reduced pressure, filter and dry to obtain tertiary aminated maleopimaric amide;
[0017] S3. Add 8-15 parts by weight of tertiary aminated maleopimaron amide and 10-16 parts by weight of benzyl chloride to N,N-dimethylformamide solvent, stir to dissolve, and react at 20-26° C. for 4-8 hours. After reaction, concentrate the solution, wash, and recrystallize to obtain hydroxy-quaternary ammonium modified maleopimaron amide.
[0018] Preferably, the preparation method of the silicone rubber-containing fracturing fluid comprises the following steps: adding silicone rubber, sulfonic acid-modified maleopimaric acid ester, hydroxyl-quaternary ammonium-modified maleopimaric acid ester, sodium salicylate and water into a reactor, stirring at 30-35° C. for 10-15 minutes, and obtaining the silicone rubber-containing fracturing fluid after completion.
[0019] 3. Beneficial technical effects
[0020] The invention adds silicone rubber, sulfonic acid modified maleopimaric acid ester, hydroxyl-quaternary ammonium modified maleopimaric acid, sodium salicylate and water into a reactor, and stirs to obtain silicone rubber-containing fracturing fluid.
[0021] Maleic anhydride pimaric acid is reacted with p-tolyl urea to introduce a new carboxyl group to obtain intermediate 1, the carboxyl group in intermediate 1 and the hydroxyl group in 1,3-bis(dimethylamino)-2-propanol are subjected to esterification reaction to introduce a tertiary amine group to obtain intermediate 2, the tertiary amine group in intermediate 2 is reacted with 1,3-propane sultone to generate a quaternary ammonium salt group to obtain sulfonic acid modified maleopimaric acid ester; the carboxyl group of intermediate 1 is reacted with thionyl chloride to obtain acyl chloride intermediate 1; the acyl chloride intermediate 1 is reacted with the secondary amine in diethanolamine to obtain tertiary aminated maleopimaric amide, the tertiary amine group in the tertiary aminated maleopimaric amide is reacted with the chlorine in benzyl chloride to generate a quaternary ammonium salt and obtain hydroxyl-quaternary ammonium modified maleopimaric amide.
[0022] The silicone rubber structure contained in the present invention contains silicon-oxygen bonds, which can improve the viscosity of the fracturing fluid and make it have good shear resistance under high temperature environment. The quaternary ammonium salt group can change the wettability of rocks and reduce damage to the formation. The benzene ring structure contained in the hydroxyl-quaternary ammonium modified maleopimaric amide improves the temperature resistance and shear resistance of the fracturing fluid. The hydroxyl group can improve the thermal stability and shear stability of the fracturing fluid, so that it can still maintain high performance under high temperature and high pressure formation conditions. The hydroxyl group in the hydroxyl-quaternary ammonium modified maleopimaric amide can form hydrogen bonds with the sulfonic acid in the sulfonic acid modified maleopimaric amide ester, and the hydrogen bonds can also enhance the viscosity of the fracturing fluid, so that it can remain stable under high temperature and high pressure conditions. DETAILED DESCRIPTION
[0023] The preparation of maleic anhydride pimaric acid was carried out with reference to the document "Synthesis of Maleic Pimaric Acid Series Derivatives" (Fine Chemicals, Vol. 22, No. 11, 2005).
[0024] The structural formula of maleic anhydride pimaric acid is:
[0025] Example 1
[0026] (1) Add maleic anhydride pimaric acid to a reactor, heat in an oil bath at 120°C for 18 min, then add p-tolyl urea under stirring, wherein the mass ratio of maleic anhydride pimaric acid to p-tolyl urea is 1:0.4, continue to react for 3 h after addition, cool to room temperature after reaction, and recrystallize twice from methanol to obtain intermediate 1;
[0027] (2) Add intermediate 1 and 1,3-bis(dimethylamino)-2-propanol to N,N-dimethylformamide solvent, stir to dissolve, and continue to add p-toluenesulfonic acid catalyst, wherein the mass ratio of intermediate 1, 1,3-bis(dimethylamino)-2-propanol and p-toluenesulfonic acid catalyst is 1.3:1:0.01, react at 90°C for 8h, and then distill under reduced pressure, filter and dry to obtain intermediate 2;
[0028] (3) Under nitrogen atmosphere, intermediate 2 and 1,3-propane sultone in a mass ratio of 1:1.4 were added to the reactor, stirred and mixed, and reacted at 20°C for 20 hours. After the reaction, the mixture was filtered, washed and dried to obtain sulfonic acid-modified maleopimaric acid ester. The reaction process of sulfonic acid-modified maleopimaric acid ester is as follows:
[0029]
[0030] (4) Add 5 parts by weight of intermediate 1 to 10 parts by weight of thionyl chloride, disperse evenly, react at 70° C. for 20 h, filter after reaction, wash and dry to obtain acyl chloride intermediate 1;
[0031] (5) Add 8 parts by weight of the acyl chloride intermediate 1 and 6 parts by weight of diethanolamine to N,N-dimethylformamide solvent, stir and dissolve, continue to add 1 part by weight of pyridine catalyst, react at 75° C. for 8 hours, and then distill under reduced pressure, filter and dry to obtain tertiary aminated maleopimaronamide;
[0032] (6) 8 parts by weight of tertiary aminated maleopimaron amide and 10 parts by weight of benzyl chloride were added to N,N-dimethylformamide solvent, stirred to dissolve, and reacted at 20° C. for 4 hours. After the reaction, the solution was concentrated, washed, and recrystallized to obtain hydroxy-quaternary ammonium modified maleopimaron amide; the reaction formula of hydroxy-quaternary ammonium modified maleopimaron amide is as follows:
[0033]
[0034] (7) Add 5 parts by weight of silicone rubber, 6 parts by weight of sulfonic acid-modified maleopimaric acid ester, 4 parts by weight of hydroxyl-quaternary ammonium-modified maleopimaric acid ester, 0.4 parts by weight of sodium salicylate, and 20 parts by weight of water into a reactor, and stir at 30° C. for 10 minutes to obtain a silicone rubber-containing fracturing fluid. Example 2
[0035] (1) Maleic anhydride pimaric acid was added to a reactor, heated in an oil bath at 140°C for 25 min, and then p-tolyl urea was added under stirring, wherein the mass ratio of maleic anhydride pimaric acid to p-tolyl urea was 1:0.6. After the addition, the reaction was continued for 4 h. After the reaction was completed, the reaction was cooled to room temperature and recrystallized from methanol for 3 times to obtain intermediate 1;
[0036] (2) Add intermediate 1 and 1,3-bis(dimethylamino)-2-propanol to N,N-dimethylformamide solvent, stir to dissolve, and continue to add p-toluenesulfonic acid catalyst, wherein the mass ratio of intermediate 1, 1,3-bis(dimethylamino)-2-propanol and p-toluenesulfonic acid catalyst is 1.5:1:0.03, react at 110°C for 12 hours, and then distill under reduced pressure, filter and dry to obtain intermediate 2;
[0037] (3) Under a nitrogen atmosphere, intermediate 2 and 1,3-propane sultone in a mass ratio of 1:1.8 were added to the reactor, the mixture was stirred and mixed, and the reaction was carried out at 25°C for 30 hours. After the reaction, the mixture was filtered, washed and dried to obtain sulfonic acid-modified maleopimaric acid ester;
[0038] (4) adding 8 parts by weight of the intermediate 1 to 15 parts by weight of thionyl chloride, dispersing the mixture evenly, reacting the mixture at 80° C. for 24 hours, filtering the mixture after the reaction, washing the mixture and drying the mixture to obtain the acyl chloride intermediate 1;
[0039] (5) Add 14 parts by weight of the acyl chloride intermediate 1 and 15 parts by weight of diethanolamine to N,N-dimethylformamide solvent, stir and dissolve, continue to add 2 parts by weight of pyridine catalyst, react at 90° C. for 14 hours, and then distill under reduced pressure, filter and dry to obtain tertiary aminated maleopimaronamide;
[0040] (6) adding 15 parts by weight of tertiary aminated maleopimaron amide and 16 parts by weight of benzyl chloride to N,N-dimethylformamide solvent, stirring to dissolve, reacting at 26° C. for 8 h, and then concentrating the solution, washing, and recrystallizing to obtain hydroxy-quaternary ammonium modified maleopimaron amide;
[0041] (7) 7 parts by weight of silicone rubber, 10 parts by weight of sulfonic acid-modified maleopimaric acid ester, 6 parts by weight of hydroxyl-quaternary ammonium-modified maleopimaric acid, 0.8 parts by weight of sodium salicylate, and 30 parts by weight of water were added into a reactor and stirred at 35° C. for 15 minutes to obtain a silicone rubber-containing fracturing fluid. Example 3
[0042] (1) Maleic anhydride pimaric acid was added to a reactor, heated in an oil bath at 130°C for 21 min, and then p-tolyl urea was added under stirring, wherein the mass ratio of maleic anhydride pimaric acid to p-tolyl urea was 1:0.5. After the addition, the reaction was continued for 3.5 h. After the reaction was completed, the reaction was cooled to room temperature and recrystallized with methanol 2.5 times to obtain intermediate 1;
[0043] (2) Add intermediate 1 and 1,3-bis(dimethylamino)-2-propanol to N,N-dimethylformamide solvent, stir to dissolve, and continue to add p-toluenesulfonic acid catalyst, wherein the mass ratio of intermediate 1, 1,3-bis(dimethylamino)-2-propanol and p-toluenesulfonic acid catalyst is 1.4:1:0.02, react at 100°C for 10 hours, and then distill under reduced pressure, filter and dry to obtain intermediate 2;
[0044] (3) Under a nitrogen atmosphere, intermediate 2 and 1,3-propane sultone in a mass ratio of 1:1.6 were added to the reactor, stirred and mixed, and reacted at 22°C for 25 h. After the reaction, the mixture was filtered, washed and dried to obtain sulfonic acid-modified maleopimaric acid ester;
[0045] (4) adding 6 parts by weight of the intermediate 1 to 12 parts by weight of thionyl chloride, dispersing the mixture evenly, reacting the mixture at 75° C. for 22 hours, filtering the mixture after the reaction, washing the mixture and drying the mixture to obtain the acyl chloride intermediate 1;
[0046] (5) Add 11 parts by weight of the acyl chloride intermediate 1 and 10 parts by weight of diethanolamine to N,N-dimethylformamide solvent, stir to dissolve, continue to add 1.5 parts by weight of pyridine catalyst, react at 82° C. for 11 hours, and then distill under reduced pressure, filter and dry to obtain tertiary aminated maleopimaronamide;
[0047] (6) adding 11 parts by weight of tertiary aminated maleopimaron amide and 13 parts by weight of benzyl chloride to N,N-dimethylformamide solvent, stirring to dissolve, reacting at 23° C. for 6 hours, and then concentrating the solution, washing, and recrystallizing to obtain hydroxy-quaternary ammonium modified maleopimaron amide;
[0048] (7) 6 parts by weight of silicone rubber, 8 parts by weight of sulfonic acid-modified maleopimaric acid ester, 5 parts by weight of hydroxyl-quaternary ammonium-modified maleopimaric acid, 0.6 parts by weight of sodium salicylate, and 25 parts by weight of water were added into a reactor and stirred at 32° C. for 12 minutes to obtain a silicone rubber-containing fracturing fluid. Example 4
[0049] (1) Add maleic anhydride pimaric acid to a reactor, heat in an oil bath at 120°C for 18 min, then add p-tolyl urea under stirring, wherein the mass ratio of maleic anhydride pimaric acid to p-tolyl urea is 1:0.4, continue to react for 3 h after addition, cool to room temperature after reaction, and recrystallize twice from methanol to obtain intermediate 1;
[0050] (2) Add intermediate 1 and 1,3-bis(dimethylamino)-2-propanol to N,N-dimethylformamide solvent, stir to dissolve, and continue to add p-toluenesulfonic acid catalyst, wherein the mass ratio of intermediate 1, 1,3-bis(dimethylamino)-2-propanol and p-toluenesulfonic acid catalyst is 1.3:1:0.01, react at 90°C for 8h, and then distill under reduced pressure, filter and dry to obtain intermediate 2;
[0051] (3) Under a nitrogen atmosphere, intermediate 2 and 1,3-propane sultone in a mass ratio of 1:1.8 were added to the reactor, the mixture was stirred and mixed, and the reaction was carried out at 25°C for 30 hours. After the reaction, the mixture was filtered, washed and dried to obtain sulfonic acid-modified maleopimaric acid ester;
[0052] (4) adding 8 parts by weight of the intermediate 1 to 15 parts by weight of thionyl chloride, dispersing the mixture evenly, reacting the mixture at 80° C. for 24 hours, filtering the mixture after the reaction, washing the mixture and drying the mixture to obtain the acyl chloride intermediate 1;
[0053] (5) Add 11 parts by weight of the acyl chloride intermediate 1 and 10 parts by weight of diethanolamine to N,N-dimethylformamide solvent, stir to dissolve, continue to add 1.5 parts by weight of pyridine catalyst, react at 82° C. for 11 hours, and then distill under reduced pressure, filter and dry to obtain tertiary aminated maleopimaronamide;
[0054] (6) adding 11 parts by weight of tertiary aminated maleopimaron amide and 13 parts by weight of benzyl chloride to N,N-dimethylformamide solvent, stirring to dissolve, reacting at 23° C. for 6 hours, and then concentrating the solution, washing, and recrystallizing to obtain hydroxy-quaternary ammonium modified maleopimaron amide;
[0055] (7) 6 parts by weight of silicone rubber, 8 parts by weight of sulfonic acid-modified maleopimaric acid ester, 5 parts by weight of hydroxyl-quaternary ammonium-modified maleopimaric acid, 0.6 parts by weight of sodium salicylate, and 25 parts by weight of water were added into a reactor and stirred at 32° C. for 12 minutes to obtain a silicone rubber-containing fracturing fluid. Example 5
[0056] (1) Maleic anhydride pimaric acid was added to a reactor, heated in an oil bath at 140°C for 25 min, and then p-tolyl urea was added under stirring, wherein the mass ratio of maleic anhydride pimaric acid to p-tolyl urea was 1:0.6. After the addition, the reaction was continued for 4 h. After the reaction was completed, the reaction was cooled to room temperature and recrystallized from methanol for 3 times to obtain intermediate 1;
[0057] (2) Add intermediate 1 and 1,3-bis(dimethylamino)-2-propanol to N,N-dimethylformamide solvent, stir to dissolve, and continue to add p-toluenesulfonic acid catalyst, wherein the mass ratio of intermediate 1, 1,3-bis(dimethylamino)-2-propanol and p-toluenesulfonic acid catalyst is 1.5:1:0.03, react at 110°C for 12 hours, and then distill under reduced pressure, filter and dry to obtain intermediate 2;
[0058] (3) Under a nitrogen atmosphere, intermediate 2 and 1,3-propane sultone in a mass ratio of 1:1.6 were added to the reactor, stirred and mixed, and reacted at 22°C for 25 h. After the reaction, the mixture was filtered, washed and dried to obtain sulfonic acid-modified maleopimaric acid ester;
[0059] (4) adding 6 parts by weight of the intermediate 1 to 12 parts by weight of thionyl chloride, dispersing the mixture evenly, reacting the mixture at 75° C. for 22 hours, filtering the mixture after the reaction, washing the mixture and drying the mixture to obtain the acyl chloride intermediate 1;
[0060] (5) Add 8 parts by weight of the acyl chloride intermediate 1 and 6 parts by weight of diethanolamine to N,N-dimethylformamide solvent, stir and dissolve, continue to add 1 part by weight of pyridine catalyst, react at 75° C. for 8 hours, and then distill under reduced pressure, filter and dry to obtain tertiary aminated maleopimaronamide;
[0061] (6) adding 8 parts by weight of tertiary aminated maleopimaron amide and 10 parts by weight of benzyl chloride to N,N-dimethylformamide solvent, stirring to dissolve, reacting at 20° C. for 4 hours, and after the reaction, concentrating the solution, washing, and recrystallizing to obtain hydroxy-quaternary ammonium modified maleopimaron amide;
[0062] (7) Add 5 parts by weight of silicone rubber, 6 parts by weight of sulfonic acid-modified maleopimaric acid ester, 4 parts by weight of hydroxyl-quaternary ammonium-modified maleopimaric acid ester, 0.4 parts by weight of sodium salicylate, and 20 parts by weight of water into a reactor, and stir at 30° C. for 10 minutes to obtain a silicone rubber-containing fracturing fluid.
[0063] Comparative Example 1
[0064] The difference between this comparative example and Example 5 is that no sulfonic acid-modified maleopimaric acid ester is added.
[0065] Comparative Example 2
[0066] Compared with Example 5, this comparative example is characterized in that no hydroxy-quaternary ammonium modified maleopimaronamide is added.
[0067] The silicone rubber-containing fracturing fluid prepared in the examples and comparative examples was added to water to prepare a simulated fracturing fluid with a concentration of 2%. After being stirred evenly, the fracturing fluid was sheared at 25°C, 80°C, and 150°C for 1-4 h, with a shear rate of 170 s -1 The apparent viscosity of the solution was measured using a rotational viscometer. The test results are shown in Table 1.
[0068] Table 1: High temperature resistance test.
[0069]
[0070] As can be seen from Table 1, compared with Comparative Examples 1-2, the viscosity of Examples 1-5 of the present invention at different temperatures changes less, indicating that they have better temperature resistance.
[0071] Refer to SYT6376-2008 "General Technical Conditions for Fracturing Fluids" and test the apparent viscosity and shear resistance at 150°C.
[0072] Table 2: Shear performance test.
[0073]
[0074] It can be seen from Table 2 that Examples 1-5 of the present invention have better shear performance than Comparative Examples 1-2.
[0075] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A fracturing fluid containing silicone rubber, characterized in that: The invention comprises the following components by weight: 5-7 parts by weight of silicone rubber, 6-10 parts by weight of sulfonic acid modified maleopimaric acid ester, 4-6 parts by weight of hydroxyl-quaternary ammonium modified maleopimaric acid amide, 0.4-0.8 parts by weight of sodium salicylate, and 20-30 parts by weight of water; The preparation method of the sulfonic acid modified maleopimaric acid ester is as follows: (1) Maleic anhydride and pimaric acid were added to the reactor, heated in an oil bath at 120-140°C for 18-25 min, and then p-tolyl urea was added under stirring. After the addition, the reaction was continued for 3-4 h. After the reaction was completed, the reaction was cooled to room temperature and recrystallized from methanol for 2-3 times to obtain intermediate 1; (2) Add intermediate 1 and 1,3-bis(dimethylamino)-2-propanol to N,N-dimethylformamide solvent, stir to dissolve, continue to add p-toluenesulfonic acid catalyst, react at 90-110°C for 8-12h, distill under reduced pressure after reaction, filter and dry to obtain intermediate 2; (3) Under a nitrogen atmosphere, add intermediate 2 and 1,3-propane sultone to a reactor, stir and mix, react at 20-25° C. for 20-30 h, filter after reaction, wash and dry to obtain sulfonic acid-modified maleopimaric acid ester; The preparation method of the hydroxyl-quaternary ammonium modified maleopimaronamide is as follows: S1. 5-8 parts by weight of intermediate 1 is added to 10-15 parts by weight of thionyl chloride, dispersed evenly, reacted at 70-80 ° C for 20-24h, filtered after the reaction, washed and dried to obtain an acyl chloride intermediate 1; S2. Add 8-14 parts by weight of the acyl chloride intermediate 1 and 6-15 parts by weight of diethanolamine to N,N-dimethylformamide solvent, stir to dissolve, continue to add 1-2 parts by weight of pyridine catalyst, react at 75-90 ° C for 8-14h, and then distill under reduced pressure, filter and dry to obtain tertiary aminated maleopimaric amide; S3. Add 8-15 parts by weight of tertiary aminated maleopimaron amide and 10-16 parts by weight of benzyl chloride to N,N-dimethylformamide solvent, stir to dissolve, and react at 20-26° C. for 4-8 hours. After reaction, concentrate the solution, wash, and recrystallize to obtain hydroxy-quaternary ammonium modified maleopimaron amide.
2. The silicone rubber-containing fracturing fluid according to claim 1, characterized in that: The mass ratio of maleic anhydride pimaric acid to p-tolyl urea in (1) is 1:0.4-0.
6.
3. The silicone rubber-containing fracturing fluid according to claim 1, characterized in that: The mass ratio of the intermediate 1, 1,3-bis(dimethylamino)-2-propanol and p-toluenesulfonic acid catalyst in (2) is 1.3-1.5:1:0.01-0.
03.
4. The silicone rubber-containing fracturing fluid according to claim 1, characterized in that: The mass ratio of the intermediate 2 to 1,3-propane sultone in (3) is 1:1.4-1.
8.
5. A method for preparing a silicone rubber-containing fracturing fluid according to any one of claims 1 to 4, characterized in that: The preparation method of the silicone rubber-containing fracturing fluid comprises the following steps: adding silicone rubber, sulfonic acid-modified maleopimaric acid ester, hydroxyl-quaternary ammonium-modified maleopimaric acid ester, sodium salicylate and water into a reactor, stirring at 30-35° C. for 10-15 minutes, and obtaining the silicone rubber-containing fracturing fluid after the stirring.
Citation Information
Patent Citations
Low-temperature-resistant fracturing fluid for oil exploitation and preparation method of fracturing fluid
CN104861955A
Maleated rosin based quaternaries cation surface active agent and method of preparing the same
CN101249400A
Preparation method of rosin-based drag reducer for shale gas exploitation
CN105601798A