A method for cleaning residual cerium oxide polishing powder of quartz photomask substrate

Through the cleaning method of cerium oxide polishing powder residue on the quartz photomask substrate, technical means such as low-concentration dispersion lotion, alkali solution and hot sulfuric acid are used to solve the problem of unclean substrate caused by polishing liquid residue and achieve efficient removal of polishing powder. Improves the cleaning effect and coating quality of photomask substrates.

CN118543595BActive Publication Date: 2024-10-22HUNAN OMNISUN INFORMATION MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411000795.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-10-22
Estimated Expiration
2044-07-25

Smart Images

  • Figure CN118543595B_ABST
    Figure CN118543595B_ABST
Patent Text Reader

Abstract

The invention discloses a method for cleaning the residual cerium oxide polishing powder of a quartz photomask substrate, comprising: pre-treating a sample; performing double-sided polishing on the sample with a low-concentration dispersed detergent; soaking the pre-treated sample in alkali solution and hot sulfuric acid in sequence; rinsing the sample soaked in hot sulfuric acid with pure water; washing the sample rinsed with pure water with alkali solution and performing ultrasonic cleaning; and performing ultrasonic pure water rinsing and drying on the sample after ultrasonic cleaning. The invention can effectively remove the residual polishing liquid, obtain a substrate without particles larger than 2 microns, and then relieve the pressure of subsequent fine cleaning, and improve the quality of the photomask substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of quartz glass cleaning, in particular to a method for cleaning residual cerium oxide polishing powder of a quartz photomask substrate. Background Art

[0002] The photomask substrate is an important raw material in pattern conversion and photolithography technology. It is obtained by plating a chrome film on a flat and clean sample and then spin-coating a layer of photoresist on the chrome film. A clean environment must be maintained throughout the production process. The photomask substrate is obtained through photolithography processes such as exposure, development, etching, and degumming to obtain a photomask. Both the preparation of the photomask substrate and the subsequent plate-making process have strong requirements for precision. Any particles on the glass substrate may cause the photolithography lines to break, resulting in pattern failure and signal distortion; particle defects are the most important indicator of process accuracy.

[0003] During the entire photomask substrate manufacturing process, the largest source of substrate particles is the residue of polishing liquid. As a mixture, polishing liquid is slightly soluble in water, in granular form, and easy to agglomerate. During the chemical mechanical polishing process, the polishing liquid needs to be in relatively uniform contact with the glass surface for polishing. After polishing, the sample is equivalent to being taken out of the polishing liquid, and there will be pieces of polishing liquid covering the glass surface. Therefore, how to remove the polishing liquid is the key to obtaining a clean substrate.

[0004] In order to obtain a high-precision coating substrate, the polished substrate must go through multiple steps such as rough cleaning and fine cleaning. If the rough cleaning effect is not good, it will put great pressure on the fine cleaning, making it difficult to obtain a substrate with high cleanliness. Summary of the invention

[0005] In view of the above-mentioned deficiencies of current mask substrates, the present invention provides a method for cleaning residual cerium oxide polishing powder of a quartz photomask substrate, which can significantly reduce the number of particles after polishing and rough washing, achieve a good rough washing effect, alleviate the pressure of subsequent fine washing, and create conditions for obtaining high-level coated products.

[0006] To achieve the above object, the embodiments of the present invention adopt the following technical solutions:

[0007] A method for cleaning residual cerium oxide polishing powder of a quartz photomask substrate, comprising:

[0008] Pre-treating the sample; including double-sided polishing of the sample with a low-concentration dispersed lotion;

[0009] The pretreated sample is sequentially immersed in an alkali solution and hot sulfuric acid, wherein the concentration of the hot sulfuric acid is not less than 98%, and the hot sulfuric acid is in a circulating state during the immersion period;

[0010] Rinse the sample soaked in hot sulfuric acid with pure water; including washing the sample with multiple pure water of decreasing temperature in sequence, wherein the first washing temperature is not less than 70 degrees and the last washing temperature is not less than 40 degrees;

[0011] The sample rinsed with pure water is cleaned with alkali solution and ultrasonically cleaned. Specifically, the sample is cleaned with alkali solution of decreasing alkali concentration, and the ultrasonic frequency is controlled from small to large to ultrasonically clean the sample successively;

[0012] The samples after ultrasonic cleaning are rinsed with ultrasonic pure water and dried, including drying the samples by hot nitrogen.

[0013] According to one aspect of the present invention, the pretreatment of the sample further comprises the following steps: rinsing the sample; brushing the double-sided polished sample; and high-pressure washing the brushed sample.

[0014] According to one aspect of the present invention, the working pressure of the high-pressure washing of the scrubbed sample is not less than 5 MPa.

[0015] According to one aspect of the present invention, the concentration of the low-concentration dispersed lotion is 0.1%-2%.

[0016] According to one aspect of the present invention, the concentration of the hot sulfuric acid is not less than 98%, the temperature range is 100-130 degrees, and the pretreated sample is immersed in the hot sulfuric acid for 30-120 minutes.

[0017] According to one aspect of the present invention, the sample is cleaned by multiple passes of pure water with successively lower temperatures, specifically: the first cleaning temperature is not lower than 70 degrees, and the last cleaning temperature is not lower than 40 degrees.

[0018] According to one aspect of the present invention, the cleaning of the sample rinsed with pure water with alkali solution and ultrasonic cleaning comprises the following steps: cleaning the sample with alkali solution of decreasing alkali concentration; and ultrasonic cleaning the sample by controlling the ultrasonic frequency from small to large.

[0019] According to one aspect of the present invention, the sample rinsed with pure water is cleaned with alkali solution and ultrasonically cleaned, specifically: the ultrasonic frequency is 28-200KHZ, the alkali solution concentration is 1%-3%, and the temperature is 30-50 degrees.

[0020] According to one aspect of the present invention, the method further comprises the following steps:

[0021] Testing the dried samples;

[0022] If the test fails, return and re-clean until the test passes;

[0023] If the test is qualified, the cleaning is qualified.

[0024] According to one aspect of the present invention, the testing of the dried samples is specifically performed by placing the cleaned samples in a dark room and testing them.

[0025] The advantages of the implementation of the present invention are: the method is relatively simple and easy to operate; the effect is good and stable and controllable, and the surface particles of the photomask substrate can be effectively reduced to improve the quality of the photomask substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0027] Figure 1 is a flow chart of the present invention;

[0028] Figure 2 The present invention is a flow chart of pre-processing samples. DETAILED DESCRIPTION

[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example

[0030] Reference Figure 1 , Figure 2 , a method for cleaning residual cerium oxide polishing powder of a quartz photomask substrate, comprising:

[0031] Step S1: pre-treat the sample.

[0032] The sample is polished with cerium oxide polishing powder before cleaning, and the processing method is chemical mechanical polishing, and the specific method is not limited to single-sided or double-sided polishing.

[0033] In this example, 60 samples (quartz substrates) were selected using cerium oxide polishing liquid as the polishing raw material and obtained through chemical mechanical polishing, and the following treatment was performed:

[0034] Step S101: Rinse the sample. Rinse the sample briefly to remove the polishing liquid visible to the naked eye.

[0035] Step S102: Double-sided polishing of the sample with a low-concentration dispersant. The sample is double-sided polished with a dispersant at a concentration of 1%. Double-sided polishing with a low-concentration dispersant uses the pressure of the upper and lower disks to make a simple polishing between the sample surface and the polishing pad. The polishing powder particles adsorbed on the sample surface will fall off or be diluted under the impact and friction of the water, and then be taken away by the water; the low-concentration dispersant helps to disperse the aggregated polishing powder particles and reduce the agglomeration of polishing powder particles on the sample.

[0036] Low-concentration dispersed detergent polishing refers to polishing the sample with a dispersed detergent instead of polishing powder. The concentration of the dispersed detergent is about 0.1%-2%, and 1% concentration is preferably selected.

[0037] The dispersed detergent adopts a circulating filtration device, and the polishing pressure is a small pressure of 0.01MPA for polishing, and the polishing time is 20 minutes.

[0038] Step S103: scrub the double-sided polished sample. The sample is scrubbed mechanically, spraying hot water on the sample surface while scrubbing the sample evenly and vigorously. In addition, the edges need to be scrubbed.

[0039] The scrubbing is performed by mechanical scrubbing with a nylon brush or a PVA sponge, and is not limited to scrubbing with normal temperature water, hot water, or a neutral detergent.

[0040] Step S104: High-pressure washing is performed on the washed samples. The samples are washed with a high-pressure water gun, the pressure of the high-pressure water gun is adjusted to 8 MPa, and pure water is used to spray evenly and forcefully.

[0041] The working pressure of the high-pressure water gun shall not be less than 5MPa.

[0042] Mechanical scrubbing and high-pressure water gun washing can separate the particle clusters and flakes adhering to the sample surface from the sample base. At the same time, scrubbing helps to clean the polishing powder at the edges.

[0043] Step S2: Soak the pretreated sample in alkaline solution and hot sulfuric acid in sequence.

[0044] The ingredients of the alkali solution include a mixture of chelates, surfactants, organic acid salts, and inorganic bases. The concentration is 10%-20%, and the pH value is 10-11. The soaking time is 30-60 minutes, preferably 45 minutes.

[0045] This embodiment uses 15% alkali solution for immersion for 45 minutes. The alkali solution used is type A, and its main components are as follows:

[0046] Potassium hydroxide (less than 5%), sodium hydroxide (less than 5%), chelating agent (1-10%),

[0047] Phosphates (less than 5%), anionic surfactants (less than 5%).

[0048] The lye solution is kept at a constant temperature of 40 degrees.

[0049] The hot sulfuric acid has a concentration of 98% or more, a temperature of 100-130 degrees, preferably 120 degrees, a soaking time of 30-120 minutes, preferably 60 minutes, and the sample is evenly thrown during the soaking; the heater is an indirect heating method, and the sulfuric acid is in a flowing state during the soaking. Preferably, the sulfuric acid is in a circulating state during the soaking.

[0050] The above samples were placed on a special Teflon cleaning basket and immersed in 120-degree hot sulfuric acid together with the cleaning basket for 60 minutes. The hot sulfuric acid was kept at a constant temperature and in an internal circulation state.

[0051] Through the alkali solution and hot sulfuric acid soaking, some stains are separated from the glass surface and dissolved or suspended in the detergent. The activity of the alkali solution is closely related to its temperature, so it is important to find a suitable temperature for soaking; since there is a layer of alkali solution on the quartz surface after the alkali solution soaking, a violent reaction will occur instantly when entering the next sulfuric acid soaking. At the same time, since the strong corrosiveness of sulfuric acid increases with the increase of temperature, the detergency and corrosiveness will gradually increase, which can quickly decompose the stubborn dirt attached to the glass surface and penetrate into the dirt to achieve a deep cleaning effect.

[0052] Step S3: Rinse the sample soaked in hot sulfuric acid with pure water. The sample is washed with multiple pure waters of decreasing temperature, and the first warm pure water washing temperature is not less than 70 degrees, and the last warm pure water washing temperature is not less than 40 degrees.

[0053] In this embodiment, the sample is rinsed with pure water for 2-3 times. The first rinse tank uses 75 degrees warm pure water, the second rinse tank uses 60 degrees warm pure water, and the third rinse tank uses 45 degrees warm pure water.

[0054] The purpose of warm water rinsing is to dissolve sulfuric acid in warm water and take it away to avoid sulfuric acid residue. There are two reasons for using warm water instead of cold water. First, if the glass soaked in high-temperature sulfuric acid is directly placed in cold water, it will crack due to thermal expansion and contraction. Therefore, it is necessary to use a method of gradually lowering the water temperature for multiple times for rinsing. Second, the solubility of sulfuric acid in water is closely related to temperature, and it is easier to dissolve sulfuric acid in warm water.

[0055] Step S4: The sample rinsed with pure water is cleaned with alkaline solution and ultrasonically cleaned.

[0056] The sample is repeatedly cleaned with alkali solution and ultrasound, the ultrasonic frequency is 28-200KHZ, the alkali solution concentration is 2%-3%, the frequency is cleaned from small to large, and the temperature is 30-50 degrees.

[0057] The sample rinsed with pure water can be cleaned with alkali solution or ultrasonically cleaned separately, or the alkali solution cleaning and ultrasonic cleaning can be used in combination, such as soaking the sample in alkali solution and ultrasonic cleaning at the same time. Preferably, the alkali solution cleaning and ultrasonic cleaning are used in combination, and the alkali solution can enhance the effect of ultrasonic cleaning, so that it can better remove residues.

[0058] This embodiment adopts four ultrasonic cleanings, and the lotion used is still type A lotion, with concentrations of 3.0%, 2.4%, 1.8%, and 1.2% respectively. The ultrasonic frequencies are all dual-frequency ultrasound, which are 28 / 40khz, 40 / 75khz, 75 / 120khz, and 120 / 175khz respectively. Each cleaning has circulation filtration in the filter element.

[0059] Step S5: rinsing and drying the ultrasonically cleaned sample with pure water.

[0060] The ultrasonic frequency is 28-200KHZ, and the overflow water volume S per minute is ≥ one-third of the volume of the tank.

[0061] Rinse with ultrasonic pure water for multiple times. This embodiment uses four tanks for pure water rinsing, the tank volume is 60L, the overflow flow is 30LPM, the first three tanks have ultrasound, which are 40khz, 120khz, and 200khz respectively, and the fourth tank has no ultrasound. Each tank has nitrogen bubbling, and its flow rate is 20LPM, 20LPM, 25LPM, and 30LPM respectively. Among them, nitrogen plays the functions of bubbling, throwing, and overflow.

[0062] The firmly adsorbed scattered particles are removed by ultrasound and rinsing. The strategy for cleaning the scattered particles is to clean the large particles first and then the small particles, so the frequency of ultrasound should be low first and then high.

[0063] Dry with hot nitrogen, place the cleaning basket together with the glass in the drying tank, blow dry the sample with hot nitrogen, the nitrogen heating temperature is 150 degrees, and the filtration accuracy is 0.003 microns.

[0064] Step S6: Test the dried samples. The main process is as follows:

[0065] The dried samples were inspected in a dark room. During the inspection, the sample surface was illuminated with a light intensity of 120,000 lux, and the inspection standard was: no particles larger than 2 microns. In addition to defects such as scratches, 50 samples obtained in the embodiment were inspected for particles, of which 49 particles met the conditions and could be released, and the other 1 needed to be reworked.

[0066] Repeat the above steps for samples that fail the test. The main process is as follows:

[0067] The product with particles that do not meet the requirements will be reprocessed according to steps S1 to S6. After confirmation, it will finally meet the expected requirements and be released.

[0068] Step S7: Perform post-process fine washing on the qualified samples

[0069] The final fine cleaning mainly removes particles below 2 microns. Generally, the product (dried) that was previously rough-cleaned is cleaned again in a finer manner. The ultrasonic cleaning generally used is mega-ultrasonic 430KHZ or above for DIP cleaning or megasonic SPIN single-chip cleaning. The required clean environment is more stringent, generally carried out in a clean workshop above CLASS100. After one or more fine cleanings, the coating can be applied only after the requirements are met. The final cleaning can only be carried out on the basis of a good rough cleaning effect.

[0070] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the art within the technical scope disclosed in the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.

Claims

1. A method for cleaning residual cerium oxide polishing powder on a quartz photomask substrate, characterized in that: include: Pre-treat the sample; It includes double-sided polishing of the sample with a low-concentration dispersed lotion; The pretreated sample is sequentially immersed in an alkali solution and hot sulfuric acid, wherein the concentration of the hot sulfuric acid is not less than 98%, and the hot sulfuric acid is in a circulating state during the immersion period; Rinse the sample soaked in hot sulfuric acid with pure water; including washing the sample with multiple pure water of decreasing temperature in sequence, wherein the first washing temperature is not less than 70 degrees and the last washing temperature is not less than 40 degrees; The sample rinsed with pure water is cleaned with alkali solution and ultrasonically cleaned. Specifically, the sample is cleaned with alkali solution of decreasing alkali concentration, and the ultrasonic frequency is controlled from small to large to ultrasonically clean the sample successively; The samples after ultrasonic cleaning are rinsed with ultrasonic pure water and dried, including drying the samples by hot nitrogen.

2. The method for cleaning residual cerium oxide polishing powder of a quartz photomask substrate according to claim 1, characterized in that: The sample pretreatment also includes the following steps: rinsing the sample; brushing the double-sided polished sample; and high-pressure washing the brushed sample.

3. The method for cleaning residual cerium oxide polishing powder of a quartz photomask substrate according to claim 2, characterized in that: The working pressure of the high-pressure washing of the scrubbed sample is not less than 5 MPa.

4. The method for cleaning residual cerium oxide polishing powder of a quartz photomask substrate according to claim 1, characterized in that: The concentration of the low-concentration dispersed lotion is 0.1%-2%.

5. The method for cleaning residual cerium oxide polishing powder of a quartz photomask substrate according to claim 1, characterized in that: The temperature range of the hot sulfuric acid is 100-130 degrees, and the soaking time of the pretreated sample in the hot sulfuric acid is 30-120 minutes.

6. The method for cleaning residual cerium oxide polishing powder of a quartz photomask substrate according to claim 1, characterized in that: The sample rinsed with pure water is cleaned with alkali solution and ultrasonically cleaned, specifically: the ultrasonic frequency is 28-200KHZ, the alkali solution concentration is 1%-3%, and the temperature is 30-50 degrees.

7. The method for cleaning residual cerium oxide polishing powder of a quartz photomask substrate according to claim 1, characterized in that: The method further comprises the following steps: testing the dried sample; if the test fails, returning and re-cleaning until the test passes; if the test passes, cleaning passes.

8. The method for cleaning residual cerium oxide polishing powder of a quartz photomask substrate according to claim 7, characterized in that: The testing of the dried samples specifically includes placing the cleaned samples in a dark room and testing them.