A battery negative electrode material for improving high-energy fast charging of power batteries and a preparation method thereof

By embedding silicon source powder into the shell powder skeleton and forming chemical bond connections, combined with silver ion reaction, the problem of silicon negative electrode material poor volume expansion and conductivity in power batteries is solved, and high-energy fast charging performance is improved and cycle stability is improved. Suitable for the field of new energy vehicles.

CN118545746BActive Publication Date: 2024-11-15湖南镕锂新材料科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410999426.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-15
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

The silicon negative electrode material has deteriorated cycle life and capacity attenuation due to volume expansion and poor conductivity in power batteries, which limits its commercial application, especially in high-energy fast charging technology, which is difficult to improve performance.

Method used

Using shell powder as a skeleton, silicon source powder is embedded in it, and chemically bonded with shell powder through silane coupling agent to form a stable three-dimensional network structure, and a continuous electron migration network is formed by combining silver ion reactions to improve structural stability and circulation. performance.

Benefits of technology

Effectively alleviates the volume changes of silicon source powder during charging and discharging, improves the high-energy fast charging performance and cycle stability of the power battery, improves the energy density and charging and discharging performance, especially maintains the power performance of the battery in low temperature environments. .

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a battery negative electrode material and a preparation method thereof for improving the high-energy fast charging of a power battery, and belongs to the technical field of negative electrode materials for new energy batteries. Among them, the preparation method of the battery negative electrode material comprises: pretreatment of shell powder; high-temperature steaming and baking the pretreated shell powder, then soaking it in water for 3-7 hours, and rinsing it with distilled water until neutral; treating silicon source powder with a silane coupling agent, mixing the treated silicon source powder with the shell powder in the previous step, stirring or vibrating it at 60-80°C for 4-6 hours; the composite material is left to stand for 3-6 hours at 20-25°C, and dried for standby use; the material processed in the previous step is put into an AgNO3 solution for reaction, and then filtered; the product is sintered to obtain a battery negative electrode material. The battery negative electrode material obtained by the above method can be applied to the field of new energy batteries, improve the high-energy fast charging effect of power batteries and effectively alleviate the volume change of silicon materials during charging and discharging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of negative electrode materials for new energy batteries, and in particular to a negative electrode material for batteries capable of improving high-energy fast charging of power batteries and a preparation method thereof. Background Art

[0002] As a type of new energy battery, power batteries play a vital role in the field of new energy vehicles and are one of the important factors driving the development of new energy vehicles. The working principle of power batteries is that when charging, lithium ions in the positive electrode move to the negative electrode through the electrolyte and embed into the negative electrode material; when discharging, lithium ions escape from the negative electrode, return to the positive electrode through the electrolyte and embed into the positive electrode material. In this process, redox reactions occur inside the battery to achieve the conversion and storage of electrical energy.

[0003] With the continuous advancement of technology and the rapid development of the market, the structure and materials of power batteries are also constantly being optimized and innovated. As a vital component of power batteries, the performance of negative electrode materials directly affects the energy density, cycle life and safety performance of the battery. At present, negative electrode materials are mainly divided into two categories: carbon-based negative electrode materials and non-carbon-based negative electrode materials. Silicon materials have the advantage of high theoretical specific capacity as negative electrodes for lithium-ion batteries, but silicon is a semiconductor with poor conductivity. The volume expansion of silicon negative electrode materials during use leads to material pulverization, resulting in poor battery cycle life and rapid capacity decay. The huge volume effect and low electrical conductivity limit the commercial application of silicon negative electrode technology. Therefore, how to combine the characteristics of silicon materials to improve the performance of power batteries in the direction of high-energy fast charging technology is exactly the demand that the power battery market is constantly expanding. Summary of the invention

[0004] In order to solve the problems mentioned in the background technology, the present invention provides a method for preparing a battery negative electrode material for improving high-energy fast charging of power batteries. The battery negative electrode material prepared by the above method uses shell powder as a skeleton, and silicon source powder is embedded therein, which effectively alleviates the volume change of the silicon source powder during the charging and discharging process; and the skeleton structure of the shell powder can provide stable support to prevent the silicon source powder from agglomerating and pulverizing during the charging and discharging process; at the same time, the biological activity and compatibility of the shell powder may help to improve the interface stability and electrochemical properties of silicon-based negative electrode materials.

[0005] Specifically:

[0006] A method for preparing a negative electrode material for improving high-energy fast charging of a power battery, the steps comprising:

[0007] Step 1, wash the shell powder, dry it, sieve it and set aside;

[0008] Step 2, steaming and baking the shell powder processed in step 1 at high temperature, soaking the steamed and baked shell powder in water for 3-7 hours, then washing with distilled water until neutral, and drying for later use;

[0009] Step 3, treating the silicon source powder with a silane coupling agent, mixing the treated silicon source powder with the shell powder treated in step 2 at a mass ratio of 1: (7-10), and stirring or shaking at 60-80° C. for 4-6 hours;

[0010] Step 4, the composite material of step 3 is placed at 20-25°C for 3-6 hours and dried for later use;

[0011] Step 5, putting the material treated in step 4 into AgNO3 solution, reacting for 10-20 minutes under stirring conditions at 30-40°C, and filtering;

[0012] Step 6: Sinter the product of step 5 to obtain a negative electrode material for a battery.

[0013] When implementing the above embodiment, preferably, in step 1, deionized water or distilled water is used to clean the shell powder to remove impurities and oil stains on the surface of the shell powder; the shell powder is sieved through a 100-150 mesh sieve.

[0014] When implementing the above embodiment, preferably, in step 2, the high temperature steaming and baking conditions are selected to be 500-600° C. for 30-50 minutes to expand the micropore diameter of the shell powder particles.

[0015] Furthermore, in step 3, the specific operation of treating the silicon source powder with a silane coupling agent is to add the silicon source powder to the silane coupling agent solution, stir evenly, react at 20-25° C. for 2-3 hours, and filter and collect the solid product.

[0016] When implementing the above embodiment, preferably, the concentration of the silane coupling agent solution is 10%-20%, and the mass ratio of the silicon source powder to the silane coupling agent solution is 1:(25-30).

[0017] When implementing the above embodiment, preferably, the silicon source powder is silicon powder or metallic silicon powder with a particle size of 0.5-1 μm.

[0018] When implementing the above embodiment, preferably, the silane coupling agent is vinyltrimethoxysilane or γ-aminopropyltriethoxysilane.

[0019] When implementing the above embodiment, preferably, the concentration of the AgNO3 solution in step 5 is 0.1%-0.15%, and the mass ratio of the material treated in step 4 to the AgNO3 solution is 1: (10-15).

[0020] When implementing the above embodiment, preferably, in step 6, the sintering temperature is 600-700° C. and the sintering time is 1-2 hours.

[0021] In addition, the present invention provides a battery negative electrode material for improving high-energy and fast charging of a power battery, which is prepared by the above-mentioned method for preparing a battery negative electrode material for improving high-energy and fast charging of a power battery.

[0022] Compared with the prior art, the present invention has the following beneficial features:

[0023] 1. The battery negative electrode material of the present invention uses shell powder, silicon source powder, silane coupling agent, metallic silver and other materials as a system to construct a three-dimensional network structure, a composite material, improves the structural stability of the material during charging and discharging, and improves the cycle performance. Its structural composition is based on the fact that the microscopic surface of the shell powder is porous and the pore size is mostly 2 to 5 μm. Silicon source powder with a particle size of 0.5-1 μm is selected to enable the silicon source powder to be embedded in the micropores of the shell powder, and the silane coupling agent is used to connect the two with chemical bonds, and the three cooperate to form a stable structure. The use of pores is beneficial to the rapid embedding and detachment of lithium ions, and the silicon material has a high theoretical specific capacity, which improves the high-energy fast charging performance of the power battery.

[0024] 2. The battery negative electrode material of the present invention is prepared by placing the composite material in an AgNO3 solution, reacting the silver ions with the functional groups on the silane coupling agent, shell powder, and silicon source powder, and forming a layer of film-like structure on the surface of the composite material after sintering, which synergistically constitutes a continuous electron migration network, reduces impedance and improves cycle performance. In addition, shell powder can achieve high ion conductivity at a lower temperature, thereby improving the energy density and charge and discharge performance of the battery, so that the power battery can improve the power performance in the northern winter environment.

[0025] 3. The battery negative electrode material of the present invention utilizes shell powder, the main component of which is calcium carbonate. In the organic electrolyte commonly used in lithium-ion batteries, calcium carbonate usually does not directly react chemically with the electrolyte and decompose, thereby ensuring the stability of the battery negative electrode material. In addition, shell powder contains rich bioactive calcium, which helps to enhance the interface bonding between the silicon-based negative electrode material and the electrolyte, thereby improving the interface stability. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] In order to facilitate those skilled in the art to implement the present invention, some of the reagents used in the embodiments and comparative examples are now described:

[0028] Shell powder: Lingshou County Zhuolei Building Materials;

[0029] Silane coupling agent: γ-aminopropyltriethoxysilane, Hangzhou Jessica Chemical;

[0030] Silicon source powder: 0.5μm silicon powder, Hebei Ruihuang Metal Materials;

[0031] AgNO3: Guangdong Xilong Chemical Industry. Example 1

[0032] A battery negative electrode material for improving high-energy fast charging of a power battery is prepared by the following steps:

[0033] Step 1, wash the shell powder with deionized water, dry it, and pass it through a 100-mesh sieve for later use;

[0034] Step 2, steaming and baking the shell powder treated in step 1 at 500° C. for 30 min, soaking the steamed shell powder in water for 3 h, then washing with distilled water until neutral, and drying for later use;

[0035] Step 3, adding the silicon source powder to the 10% silane coupling agent solution at a mass ratio of 1:25, stirring evenly, reacting at 20°C for 2h, filtering and collecting the solid product, mixing the treated silicon source powder with the shell powder treated in step 2 at a mass ratio of 1:7, and stirring or shaking at 60°C for 4h;

[0036] Step 4, the composite material of step 3 is placed at 20°C for 3 hours and dried for later use;

[0037] Step 5, the material treated in step 4 is put into a 0.1% AgNO3 solution at a mass ratio of 1:10, reacted at 30°C with stirring for 10 minutes, and filtered;

[0038] Step 6: Sinter the product of step 5 at 600° C. for 1 hour to obtain a battery negative electrode material. Example 2

[0039] A battery negative electrode material for improving high-energy fast charging of a power battery is prepared by the following steps:

[0040] Step 1, wash the shell powder with deionized water, dry it and pass it through a 150-mesh sieve for later use;

[0041] Step 2, steaming and baking the shell powder treated in step 1 at 600° C. for 50 min, soaking the steamed shell powder in water for 7 h, then washing with distilled water until neutral, and drying for later use;

[0042] Step 3, adding the silicon source powder to the 20% silane coupling agent solution at a mass ratio of 1:30, stirring evenly, reacting at 25°C for 3 hours, filtering and collecting the solid product, mixing the treated silicon source powder with the shell powder treated in step 2 at a mass ratio of 1:10, and stirring or oscillating at 80°C for 6 hours;

[0043] Step 4, the composite material of step 3 is placed at 25°C for 6 hours and dried for later use;

[0044] Step 5, the material treated in step 4 is put into a 0.15% AgNO3 solution at a mass ratio of 1:15, reacted at 40°C with stirring for 20 minutes, and filtered;

[0045] Step 6: Sinter the product of step 5 at 700° C. for 2 h to obtain a battery negative electrode material. Example 3

[0046] A battery negative electrode material for improving high-energy fast charging of a power battery is prepared by the following steps:

[0047] Step 1, wash the shell powder with deionized water, dry it, and pass it through a 100-mesh sieve for later use;

[0048] Step 2, steaming and baking the shell powder treated in step 1 at 522° C. for 30 min, soaking the steamed shell powder in water for 3 h, then washing with distilled water until neutral, and drying for later use;

[0049] Step 3, adding the silicon source powder to the 15% silane coupling agent solution at a mass ratio of 1:26, stirring evenly, reacting at 22°C for 2h, filtering and collecting the solid product, mixing the treated silicon source powder with the shell powder treated in step 2 at a mass ratio of 1:8, and stirring or oscillating at 61°C for 4h;

[0050] Step 4, the composite material of step 3 is placed at 24°C for 5 hours and dried for later use;

[0051] Step 5, the material treated in step 4 is put into a 0.1% AgNO3 solution at a mass ratio of 1:12.5, reacted at 35°C with stirring for 10 minutes, and filtered;

[0052] Step 6: Sinter the product of step 5 at 610° C. for 1 hour to obtain a battery negative electrode material. Example 4

[0053] A battery negative electrode material for improving high-energy fast charging of a power battery is prepared by the following steps:

[0054] Step 1, wash the shell powder with deionized water, dry it, and pass it through a 100-mesh sieve for later use;

[0055] Step 2, steaming and baking the shell powder treated in step 1 at 551° C. for 40 min, soaking the steamed shell powder in water for 5 h, then washing with distilled water until neutral, and drying for later use;

[0056] Step 3, adding the silicon source powder to the 15% silane coupling agent solution at a mass ratio of 1:25, stirring evenly, reacting at 22.1°C for 2h, filtering and collecting the solid product, mixing the treated silicon source powder with the shell powder treated in step 2 at a mass ratio of 1:8, and stirring or oscillating at 62.1°C for 6h;

[0057] Step 4, the composite material of step 3 is placed at 22.2°C for 4 hours and dried for later use;

[0058] Step 5, the material treated in step 4 is put into a 0.15% AgNO3 solution at a mass ratio of 1:13, reacted at 37.5°C with stirring for 15 minutes, and filtered;

[0059] Step 6: Sinter the product of step 5 at 698° C. for 1 hour to obtain a battery negative electrode material. Example 5

[0060] A battery negative electrode material for improving high-energy fast charging of a power battery is prepared by the following steps:

[0061] Step 1, wash the shell powder with deionized water, dry it and pass it through a 140-mesh sieve for later use;

[0062] Step 2, steaming and baking the shell powder treated in step 1 at 599° C. for 30 min, soaking the steamed shell powder in water for 6 h, then washing with distilled water until neutral, and drying for later use;

[0063] Step 3, adding the silicon source powder to the 15% silane coupling agent solution at a mass ratio of 1:28, stirring evenly, reacting at 25°C for 2 hours, filtering and collecting the solid product, mixing the treated silicon source powder with the shell powder treated in step 2 at a mass ratio of 1:9, and stirring or shaking at 75°C for 4 hours;

[0064] Step 4, the composite material of step 3 is placed at 24.9°C for 3 hours and dried for later use;

[0065] Step 5, the material treated in step 4 is put into a 0.14% AgNO3 solution at a mass ratio of 1:13, reacted at 37°C with stirring for 15 minutes, and filtered;

[0066] Step 6: Sinter the product of step 5 at 700° C. for 1 hour to obtain a battery negative electrode material.

[0067] Comparative Example 1

[0068] A battery negative electrode material is prepared by the following steps:

[0069] Step 1, wash the shell powder with deionized water, dry it, and pass it through a 100-mesh sieve for later use;

[0070] Step 2, steaming and baking the shell powder treated in step 1 at 500° C. for 30 min, soaking the steamed shell powder in water for 3 h, then washing with distilled water until neutral, and drying for later use;

[0071] Step 3, mixing the silicon source powder and the shell powder treated in step 2 in a mass ratio of 1:7, and stirring or shaking at 60° C. for 4 hours;

[0072] Step 4, the composite material of step 3 is placed at 20°C for 3 hours and dried for later use;

[0073] Step 5, the material treated in step 4 is put into a 0.1% AgNO3 solution at a mass ratio of 1:10, reacted at 30°C with stirring for 10 minutes, and filtered;

[0074] Step 6: Sinter the product of step 5 at 600° C. for 1 hour to obtain a battery negative electrode material.

[0075] Performance Test:

[0076] The battery negative electrode materials of Examples 1-5 and Comparative Example 1 were used to prepare batteries for testing. The battery process includes: using N-methylpyrrolidone as a solvent, adding negative electrode material, conductive carbon black, and binder LA132, the amount ratio of negative electrode material: conductive carbon black: LA132: solvent is 90g: 1g: 5g: 200mL, stirring and slurrying, coating on copper foil, drying and rolling to obtain the negative electrode; the electrolyte is 1M LiPF6+EC: DEC: DMC=1:1:1 (volume ratio); the metal lithium sheet is the counter electrode; the diaphragm is a polypropylene (PP) film; and the button half-cell is assembled in an argon-filled glove box. Using the LAND battery test system, the charge and discharge performance test was carried out at a rate of 2C.

[0077] The test results are shown in the following table:

[0078] First charge capacity (mAh / g) First discharge capacity (mAh / g) Capacity after 100 cycles (mAh / g) Lithium insertion rate (SOC%) Example 1 510.33 432.53 367.67 75.8 Example 2 507.58 429.06 360.41 76.2 Example 3 532.14 433.86 360.10 79.7 Example 4 519.53 435.16 369.88 76.5 Example 5 522.84 413.68 347.49 77.4 Comparative Example 1 457.33 365.71 255.27 50.1

[0079] It can be seen from the data in the above table that the negative electrode materials of Examples 1-5 of the present invention have the effect of high energy fast charging when applied to the battery, and have excellent cycle performance. Compared with the examples, no silane coupling agent is introduced into the system of Comparative Example 1, resulting in its capacity and lithium insertion rate being inferior to those of the examples. This proves that there is a close synergistic effect between the components in the system of the present invention.

[0080] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a negative electrode material for improving high-energy fast charging of a power battery, characterized in that: The steps include: Step 1, wash the shell powder, dry it, sieve it and set aside; Step 2, steaming and baking the shell powder processed in step 1 at high temperature, soaking the steamed and baked shell powder in water for 3-7 hours, then washing with distilled water until neutral, and drying for later use; Step 3, treating the silicon source powder with a silane coupling agent, mixing the treated silicon source powder with the shell powder treated in step 2 at a mass ratio of 1: (7-10), and stirring or shaking at 60-80° C. for 4-6 hours; Step 4, the composite material of step 3 is placed at 20-25°C for 3-6 hours and dried for later use; Step 5, putting the material treated in step 4 into AgNO3 solution, reacting for 10-20 minutes under stirring conditions at 30-40°C, and filtering; Step 6: Sinter the product of step 5 to obtain a negative electrode material for a battery.

2. The method for preparing a negative electrode material for improving high-energy fast charging of a power battery according to claim 1, characterized in that: In step 1, the shell powder is washed with deionized water or distilled water; the shell powder is passed through a 100-150 mesh sieve.

3. The method for preparing a negative electrode material for improving high-energy fast charging of a power battery according to claim 1, characterized in that: In step 2, the high temperature steaming and baking conditions are selected to be 500-600°C for 30-50 minutes.

4. The method for preparing a negative electrode material for improving high-energy fast charging of a power battery according to claim 1, characterized in that: The specific operation of treating the silicon source powder with the silane coupling agent in step 3 is to add the silicon source powder to the silane coupling agent solution, stir evenly, react at 20-25° C. for 2-3 hours, and filter and collect the solid product.

5. The method for preparing a negative electrode material for improving high-energy fast charging of a power battery according to claim 4, characterized in that: The concentration of the silane coupling agent solution is 10%-20%, and the mass ratio of the silicon source powder to the silane coupling agent solution is 1: (25-30).

6. The method for preparing a negative electrode material for improving high-energy fast charging of a power battery according to claim 1, characterized in that: The silicon source powder is selected from silicon powder or metallic silicon powder, and the particle size is 0.5-1 μm.

7. The method for preparing a negative electrode material for improving high-energy fast charging of a power battery according to claim 1, characterized in that: The silane coupling agent is vinyltrimethoxysilane or γ-aminopropyltriethoxysilane.

8. The method for preparing a negative electrode material for improving high-energy fast charging of a power battery according to claim 1, characterized in that: The concentration of the AgNO3 solution in step 5 is 0.1%-0.15%, and the mass ratio of the material treated in step 4 to the AgNO3 solution is 1: (10-15).

9. The method for preparing a negative electrode material for improving high-energy fast charging of a power battery according to claim 1, characterized in that: In step 6, the sintering temperature is 600-700° C. and the sintering time is 1-2 h.

10. A negative electrode material for improving the high energy and fast charging of a power battery, characterized in that it is prepared by the method for preparing the negative electrode material for improving the high energy and fast charging of a power battery as claimed in any one of claims 1 to 9.