A C21 dibasic acid synthesized epoxy resin emulsifier polymer and preparation method
By introducing C21 dibasic acid structure into epoxy resin, the freeze-thaw stability and flash rust problems of aqueous epoxy emulsion are solved, and the fluidity and anti-rust properties are achieved in low temperature environments, avoiding the addition of anti-stroke rust agents. It is required to improve the freeze-thaw stability and flash rust inhibition of the paint.
Patent Information
- Application Number
- CN202411026500.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-30
AI Technical Summary
The unstable and flash rust problems of water-based epoxy emulsion in low temperature environments lead to construction difficulties and corrosion of metal substrates. The existing technology is difficult to solve the problems of freeze-thaw stability and flash rust at the same time, especially the freeze-thaw of solid epoxy emulsions. Poor stability.
Using C21 dibasic acid to synthesize epoxy resin emulsifier polymers. By introducing C21 dibasic acid structure with unique properties, it reduces VOC, improves freeze-thaw stability and anti-rust properties, and uses polar groups and polyether structures to low temperatures. Maintain fluidity under the slightest risk, and avoid adding anti-flash rust agent.
The freeze-thaw stability and flash rust inhibition of epoxy emulsion in low temperature environments are achieved, the fluidity is maintained, the risk of rust is reduced, and the construction and corrosion resistance of the paint is improved.
Smart Images

Figure SMS_2 
Figure SMS_3 
Figure QLYQS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of emulsifiers, and in particular relates to a C21 dibasic acid synthesized epoxy resin emulsifier polymer and a preparation method thereof. Background Art
[0002] Waterborne epoxy resin emulsions are widely used in waterborne industrial anti-corrosion coatings, composite materials, adhesives, flooring and other fields. The importance of emulsifiers is self-evident. Its performance mainly depends on the emulsification method and the structure of the emulsifier. The main epoxy emulsifiers are divided into three categories: anionic, cationic and non-ionic. Among them, the reactive non-ionic emulsifiers in the non-ionic type have gradually become the most important part of the waterborne epoxy market due to their excellent emulsification, dispersion, low foaming, ability to participate in reactions and anti-migration after curing. The current mainstream waterborne epoxy emulsions are mainly prepared by phase inversion.
[0003] When water-based epoxy emulsion is used, there are technical problems such as poor freeze-thaw stability of solid epoxy emulsion and flash rust of water-based epoxy coating. For example, in a low temperature environment (<0°C), the epoxy emulsion will agglomerate after freezing and thawing and cannot be restored to a uniform state, resulting in the inability to construct. Or when the moisture content of the epoxy emulsion is high, it is directly applied to the metal substrate as a coating. The latent heat of volatilization of water is high, and the paint film dries slowly even at room temperature, causing water to stay on the metal substrate for a long time, making the metal substrate very prone to rust.
[0004] In order to achieve application, the current method to solve freeze-thaw and flash rust is mainly to add more diluents (solvents) and additional anti-flash rust agents, which will cause VOC to exceed the standard and increase the cost of coatings.
[0005] Patent document CN110240711B describes a preparation method for introducing polyether segments and phosphate structures into epoxy structures, which can effectively improve the rheological properties and corrosion resistance of epoxy emulsions; Patent CN109627448B uses tris (2-hydroxyethyl) isocyanurate, polyethylene glycol, neodecanoic acid glycidyl ester and epoxy resin to prepare a non-ionic epoxy emulsifier. Due to the introduction of large sterically hindered decanoic acid, the entanglement of PEG long chains is hindered, allowing them to stretch freely in the water phase, thereby improving the stability of water-based epoxy emulsions; However, these technical methods cannot solve the freeze-thaw stability of epoxy emulsions, especially the poor freeze-thaw stability of solid epoxy emulsions, and the problem of flash rust of water-based epoxy coatings. Summary of the invention
[0006] In order to solve the above technical problems, the present invention provides a C21 dibasic acid synthesized epoxy resin emulsifier polymer and a preparation method thereof. The C21 dibasic acid structure with unique properties is introduced into the epoxy resin, which not only realizes the freeze-thaw stability of the epoxy emulsion under low VOC, but also has the unique anti-rust and good low-temperature fluidity of the structure, so that the epoxy emulsion prepared by using the emulsifier has the unique advantages of no need to add anti-flash rust agent, high solid and low viscosity, and good fluidity even below 5°C in winter, and no need for more co-solvents.
[0007] The present invention solves the above technical problems by using a C21 dibasic acid to synthesize an epoxy resin emulsifier polymer, characterized in that the emulsifier polymer has the following structure:
[0008] ,
[0009] Wherein: R = bisphenol A structure or phenolic epoxy structure in epoxy resin, m,n = 55~80.
[0010] The emulsifier polymer in the present invention is a C21 dibasic acid nonionic waterborne epoxy emulsifier polymer, which has more polar groups and longer hydrocarbon chains. The polar groups in the emulsion made from the emulsifier can be directionally adsorbed on the oil-metal interface by relying on the Coulomb force or chemical bond, reducing the intrusion of corrosive media such as oxygen and water into the metal surface, and reducing the probability and rate of rust.
[0011] The present invention provides a method for preparing a C21 dibasic acid-synthesized epoxy resin emulsifier polymer, comprising the following steps:
[0012] (1) Add C21 dibasic acid and epoxy resin or phenolic epoxy resin into a reaction kettle and stir evenly. After heating to 90°C, add a catalyst and react at 90-95°C until the acid value is close to zero;
[0013] (2) Add an alkali metal catalyst, vacuum dehydrate, then introduce ethylene oxide gas after nitrogen replacement, maintain a certain pressure, and react at 90-140°C to a certain molecular weight;
[0014] In the above two steps, the appropriate temperature is important. If the reaction degree is insufficient at low temperature, the molecular weight will not meet the design requirements. If the temperature is too high, it will lead to technical problems such as violent and uncontrollable reaction and wide molecular weight distribution.
[0015] (3) Cool down to 25-35°C and use a small amount of dry ice to neutralize the emulsified system to obtain the emulsifier polymer.
[0016] In the optimized solution, the mass ratio of the C21 dibasic acid, epoxy resin or phenolic epoxy resin, catalyst and alkali metal catalyst is 353:760-1040:1.2-1.3:2-2.5.
[0017] The catalyst in step (1) is one or more of triphenylphosphine, tetraethylammonium bromide and tetrabutylammonium bromide.
[0018] The epoxy resin in step (1) is one or more of epoxy resins E51, E44, F-51 or F-44.
[0019] In the step (2), the alkali metal catalyst is KOH and / or a metal complex.
[0020] The metal catalyst is KOH or a metal complex, and step (2) in the preparation method is specifically as follows:
[0021] Add KOH or metal complex, vacuum dehydration; then introduce ethylene oxide gas after nitrogen replacement, maintain a certain pressure, react at 90-120℃ for 1-3h to cap;
[0022] Or KOH and a metal complex, step (2) in the preparation method is specifically as follows:
[0023] Add DMC bimetallic catalyst and vacuum dehydrate; then introduce ethylene oxide gas after nitrogen replacement, maintain a certain pressure, and react at 135-140°C for 1-3h; cool to 100°C, add KOH and continue to introduce ethylene oxide gas, maintain a certain pressure, and react at 90-120°C for 1-3h to cap.
[0024] The final end-capping operation is carried out at 90-120°C for 1-3 hours. If the temperature is lower than this, the molecular weight will be too low, and if the temperature is higher than this, the reaction will be uncontrollable.
[0025] The certain molecular weight in the step (2) is 6000-8000.
[0026] The vacuum dehydration in step (2) is carried out at a temperature of 90-110° C. for 1-2 hours.
[0027] The pressure in step (2) is 0.2-0.4 MPa, and 0.3 MPa in the optimized solution.
[0028] In the step (3), the temperature is lowered to 30°C.
[0029] The mass ratio of the small amount of dry ice, C21 dibasic acid and dry ice is 353:5-7.
[0030] In the present invention, ethylene oxide gas is introduced after nitrogen replacement. Nitrogen is an inert gas and does not participate in the reaction. After introduction, carbon dioxide and other gas components that interfere with the reaction can be blown out to protect the reaction process. Ethylene oxide reacts with hydroxyl groups under the action of a catalyst to open the ring, gradually polymerizes, generates a hydrophilic polyether structure, and increases the molecular weight. The reaction to an acid value close to zero allows the carboxyl group of the dibasic acid to react nearly completely, does not participate in subsequent reactions and generates by-products, and makes the product structure conform to the designed route. A small amount of dry ice is used to neutralize the emulsified system to neutrality, which plays a role in neutralizing the alkaline catalyst and preventing it from slowly reacting with the epoxy group and affecting the stability of the emulsion.
[0031] In the polymer of the present invention, the C21 dibasic acid structure provides freeze-thaw stability and anti-flash rust function, the epoxy resin structure provides hydrophobicity, compatibility and reactivity; the polyether structure provides hydrophilicity and emulsification and dispersibility, ensuring that the epoxy emulsion has a smaller particle size; the high epoxy functionality of the phenolic epoxy resin provides better heat resistance, water resistance and chemical resistance. DETAILED DESCRIPTION
[0032] The present invention is further described below in conjunction with specific embodiments:
[0033] Embodiment 1:
[0034] (1) Add 353 g C21 dibasic acid and 760 g E51 epoxy resin to a clean reactor, stir and heat to 90 °C, add 1.2 g triphenylphosphine, continue to react at 95 °C for 5 h, take a sample and test the acid value to be less than 0.5;
[0035] The carboxyl group of C21 dibasic acid can open the epoxy ring, making the two ends of the emulsifier lipophilic, and the hydroxyl group and ethylene oxide after the epoxy ring opening extend the chain to generate a hydrophilic polyether segment, thus achieving water-based properties. Compared with other carbon atoms other than 21, the carbon number is small, the carbon-hydrogen bond segment in the emulsifier structure is short, and the freeze-thaw performance will be worse.
[0036] In step (1), the reaction temperature is lower than the temperature in the present invention, the reaction degree is insufficient, the molecular weight does not meet the design requirements, the polyether chain segment becomes shorter, the hydrophilicity decreases, and the emulsification effect becomes worse. If the temperature is too high, the reaction will be violent and uncontrollable, gelation will be easily generated, and the molecular weight distribution will be wide.
[0037] (2) Add 2g KOH and vacuum dehydrate at 90℃ for 2h; then introduce ethylene oxide gas after nitrogen replacement, maintain the pressure at 0.3MPa, and react at 90℃ for 2h;
[0038] Step (2) is to polymerize ethylene oxide to generate hydrophilic polyether segments. Without this step, there will be no hydrophilic end but only lipophilic end, and epoxy will definitely not be emulsified, so no verification is required.
[0039] The alkali metal acts as a catalyst, catalyzing the ring opening of ethylene oxide and the reaction of hydroxyl groups on the product of the previous step to gradually polymerize to form polyether segments, thereby increasing the molecular weight and hydrophilicity.
[0040] (3) The reaction kettle was cooled to 30°C and 5 g of dry ice was added to neutralize the system to obtain C21 dibasic acid nonionic waterborne epoxy emulsifier A.
[0041] In the traditional method, the epoxy resin is first modified with alcohol and then reacted with dibasic acid, but the effect of the present invention cannot be obtained. The characteristic of the emulsifier in the present invention is the introduction of C21 dibasic acid structure. The longer hydrocarbon chain segment in the dibasic acid structure allows the final emulsion to obtain anti-freeze-thaw performance and flash rust performance, which are not available in polyethylene glycol and phthalic anhydride modified epoxy emulsifiers.
[0042] Embodiment 2:
[0043] (1) Add 353 g of C21 dibasic acid and 920 g of E44 epoxy resin to a clean reactor, stir and heat to 90 °C, add 1.2 g of triphenylphosphine, continue to react at 90 °C for 5 h, and take samples to test the acid value to be less than 0.5;
[0044] (2) Add 2.5 g KOH and vacuum dehydrate at 90 °C for 2 h; then introduce ethylene oxide gas after nitrogen replacement, maintain the pressure at 0.3 MPa, and react at 120 °C for 2 h;
[0045] (3) The reaction kettle was cooled to 30°C and 7 g of dry ice was added to neutralize the system to obtain C21 dibasic acid nonionic waterborne epoxy emulsifier B.
[0046] Embodiment 3:
[0047] (1) Add 353 g C21 dibasic acid and 1040 g F-44 phenolic epoxy resin to a clean reactor, stir and heat to 90 °C, add 1.2 g triphenylphosphine, continue to react at 90 °C for 5 h, take a sample and test the acid value to be less than 0.5;
[0048] (2) Add 2.5 g KOH and vacuum dehydrate at 90 °C for 2 h; then introduce ethylene oxide gas after nitrogen replacement, maintain the pressure at 0.3 MPa, and react at 110 °C for 2 h;
[0049] (3) The reaction kettle was cooled to 30°C, and 7 g of dry ice was added to neutralize the system to obtain C21 dibasic acid nonionic waterborne epoxy emulsifier C.
[0050] Embodiment 4:
[0051] (1) Add 353 g C21 dibasic acid and 900 g F-51 phenolic epoxy resin to a clean reactor, stir and heat to 90 °C, add 1.2 g triphenylphosphine, continue to react at 93 °C for 5 h, and take samples to test the acid value to be less than 0.5;
[0052] (2) Add 2.3 g KOH and vacuum dehydrate at 90 degrees for 2 hours; then introduce ethylene oxide gas after nitrogen replacement, maintain the pressure at 0.3 MPa, and react at 100 degrees for 2 hours;
[0053] (3) The reaction kettle was cooled to 30°C, and 7 g of dry ice was added to neutralize the system to obtain C21 dibasic acid nonionic waterborne epoxy emulsifier D.
[0054] Embodiment 5:
[0055] (1) Add 353 g C21 dibasic acid and 760 g E51 epoxy resin to a clean reactor, stir and heat to 90 °C, add 1.3 g tetraethylammonium bromide, continue to react at 92 °C for 5 h, take a sample and test the acid value to be less than 0.5;
[0056] (2) Add 2g KOH and vacuum dehydrate at 90℃ for 3h; then introduce ethylene oxide gas after nitrogen replacement, maintain the pressure at 0.3MPa, and react at 150℃ for 2h;
[0057] (3) The reaction kettle was cooled to 30°C, and 5 g of dry ice was added to neutralize the system to obtain C21 dibasic acid nonionic waterborne epoxy emulsifier E.
[0058] Embodiment 6:
[0059] (1) Add 353 g of C21 dibasic acid and 920 g of E44 epoxy resin to a clean reactor, stir and heat to 90 °C, add 1.2 g of triphenylphosphine, continue to react at 95 °C for 5 h, and take a sample to test the acid value to be less than 0.15;
[0060] (2) Add 0.03 g of DMC bimetallic catalyst and vacuum dehydrate at 100 °C for 1 h; then introduce ethylene oxide gas after nitrogen replacement, maintain the pressure at 0.3 MPa, and react at 140 °C for 2 h;
[0061] (3) Cool down to 100°C, add 2g KOH and continue to introduce ethylene oxide gas, maintain the pressure at 0.3MPa, and react at 90-120°C for 2h to cap the reaction;
[0062] (4) The reaction kettle was cooled to 30°C, and 7 g of dry ice was added to neutralize the system to obtain C21 dibasic acid nonionic waterborne epoxy emulsifier F.
[0063] Compared with the catalysts in the first five examples, the DMC bimetallic catalyst in Example 6 can make the molecular weight distribution more uniform and the effect is better.
[0064] Test 1
[0065] The above emulsifier polymers were respectively prepared according to the following formulas through phase inversion process to prepare water-based epoxy emulsions, with an emulsification temperature of 70 degrees, a water addition time of 3 hours, and a 60mm dispersion disk speed of 2000rpm; see Table 1 below
[0066] Table 1
[0067]
[0068] The performance of the prepared epoxy emulsion was investigated by testing its viscosity, solid content, particle size, freeze-thaw stability and flash rust inhibition. The results are shown in Table 2 below:
[0069] Table 2
[0070]
[0071] As can be seen from Table 2 above, the above epoxy emulsion can undergo at least 4 cycles of freeze-thaw cycles, indicating that the freeze-thaw performance is good, and the flash rust inhibition is all passed, indicating that the above emulsion has good anti-flash rust performance.
[0072] The freeze-thaw stability in the above table is tested according to GB / T 9268-2008 "Freeze-thaw resistance test of latex paint", and the method is as follows:
[0073] The epoxy emulsion was placed in a 500ml sealed container with a filling volume of 2 / 3, placed in a -18℃±2℃ environment for 18 hours, then taken out and placed in a room temperature environment for thawing for 6 hours. This is a complete freeze-thaw cycle. After each cycle, open the container to observe whether there are lumps, coagulation and separation. If there are no such phenomena, proceed to the next cycle until an abnormality occurs and the cycle is terminated and recorded.
[0074] The flash rust inhibition in the above table is tested according to HGT 4759-2014 "Waterborne Epoxy Anticorrosive Coatings" and the method is as follows:
[0075] The curing agent and the above emulsion are mixed in a paint according to a 1:1 amine hydrogen equivalent ratio, and a 50±2μm paint film is applied on a sandblasted steel plate with a specification of 150×70×(0.8-1.5)mm.
[0076] Place the test plate horizontally for 24 hours and observe whether there is rust on the paint film surface. Then, immediately soak the test plate in butanone [or xylene: butanol (volume ratio) = 3:1] solvent to remove the paint film (if necessary, wooden tools can be used) and observe whether there are rust spots on the substrate. If there is no rust on the paint film surface and no rust spots on the substrate, it indicates that the flash rust inhibition is qualified and is evaluated as "normal", that is, passed. Otherwise, it is evaluated as "unqualified", that is, failed.
[0077] The above implementation / test examples are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A C21 dibasic acid synthesized epoxy resin emulsifier polymer, characterized in that: The emulsifier polymer structure is as follows: ; Where: R = bisphenol A structure or phenolic epoxy structure in epoxy resin, m, n = 55∽80; The preparation method comprises the following steps: (1) Add C21 dibasic acid and epoxy resin into a reaction kettle and stir evenly. After heating to 90°C, add a catalyst and react at 90-95°C until the acid value is close to zero; the catalyst is one or more of triphenylphosphine, tetraethylammonium bromide, and tetrabutylammonium bromide; (2) adding an alkali metal catalyst, vacuum dehydration, and then introducing ethylene oxide gas after nitrogen replacement, maintaining a certain pressure, and reacting at 90-140° C. to a molecular weight of 6000-8000; the alkali metal catalyst is KOH or / and a metal complex; the mass ratio of C21 dibasic acid, epoxy resin, catalyst and alkali metal catalyst is 353:760-1040:1.2-1.3:2-2.5; (3) Cool down to 25-35°C and use a small amount of dry ice to neutralize the emulsified system to obtain the emulsifier polymer.
2. The method for preparing a C21 dibasic acid synthesized epoxy resin emulsifier polymer according to claim 1, characterized in that: The epoxy resin in step (1) is one or more of epoxy resins E51, E44, F-51 or F-44.
3. The method for preparing a C21 dibasic acid synthesized epoxy resin emulsifier polymer according to claim 2, characterized in that: The alkali metal catalyst is KOH or a metal complex, and the step (2) is specifically as follows: Add KOH or metal complex, vacuum dehydration; then introduce ethylene oxide gas after nitrogen replacement, maintain a certain pressure, and react at 90-120°C for 1-3h.
4. The method for preparing a C21 dibasic acid-synthesized epoxy resin emulsifier polymer according to claim 2, characterized in that: The alkali metal catalyst is KOH and a metal complex, and the step (2) is specifically as follows: Add DMC bimetallic catalyst and vacuum dehydrate; then introduce ethylene oxide gas after nitrogen replacement, maintain a certain pressure, and react at 135-140°C for 1-3h; cool to 100°C, add KOH and continue to introduce ethylene oxide gas, maintain a certain pressure, and react at 90-120°C for 1-3h to cap.