A method for improving the performance of aramid insulating pull rod based on interface functional modification
By introducing polar groups and graphene oxide on the surface of aramid fibers, a multi-scale functional layer on the interface is constructed, which solves the problem of improving mechanical and insulation performance of insulating pull rods in the prior art, and realizes the "mechanical-electric" performance of insulating pull rods. Coordinated improvement improves the reliability of the equipment.
Patent Information
- Application Number
- CN202410753537.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-06-12
AI Technical Summary
The prior art is difficult to simultaneously improve the mechanical properties and insulation properties of aramid fiber reinforced epoxy composite materials, resulting in discharge accidents that are prone to insulated pull rods under high pressure strong fields.
By introducing polar groups on the surface of the aramid fiber, immersing them in alkaline graphene oxide solution, plasma discharge pretreatment and chemical modification, combining nanographene oxide functional fillers, building a multi-scale functional layer on the interface to enhance the fiber Combines strength and insulation properties with the interface with the substrate.
It significantly improves the mechanical and insulation performance of the insulated pull rod, enhances the interface shear strength and AC breakdown strength, and reduces the conductivity and improves the reliability of the equipment.
Smart Images

Figure CN118546414B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high-voltage equipment, and in particular to a method for improving the performance of an aramid insulating pull rod based on interface functional modification. Background Art
[0002] Aramid fiber reinforced epoxy composites (AFRC) are widely used in the field of electrical engineering due to their high specific strength, excellent insulation properties and corrosion resistance. As a key action insulating component in the gas insulated switchgear (GIS) circuit breaker, the insulating rod made of aramid fiber reinforced epoxy composite plays the role of transmitting mechanical loads between high-potential components and grounded parts. Therefore, the insulating rod usually needs to withstand not only large dynamic mechanical loads, but also high voltage and strong fields during operation. However, the chemical inertness and high surface crystallinity of aramid fiber limit its effective combination with epoxy resin, resulting in insufficient impregnation with epoxy resin, prone to defects such as weak interface bonding and pores, which may cause discharge accidents during operation. Therefore, enhancing the interface bonding between aramid fiber and epoxy resin by modification is the key to improving the performance of insulating rods. There are many interface modification methods, including surface oxidation treatment, chemical etching, surface grafting of polar groups, etc. However, most of the interface modification methods focus on how to improve the mechanical properties of aramid fiber reinforced epoxy composite materials, and there are few studies on how to improve their mechanical and insulation properties at the same time. The relevant methods are not suitable for improving the reliability of electrical equipment such as insulating rods. In view of the above problems, the present invention provides a method for improving the performance of aramid insulating rods based on interface functional modification. Summary of the invention
[0003] The purpose of the present invention is to provide a method for improving the performance of aramid insulating rods based on interface functionalization modification, construct an interface multi-scale functional layer, improve the interface compatibility and insulation strength between aramid fibers and epoxy resin matrix in insulating rods for GIS circuit breakers, and obtain interface functionalized aramid insulating rods, thereby solving the problem that the existing modification methods cannot simultaneously improve the mechanical properties and insulation properties of aramid fiber reinforced epoxy composite materials, and realizing the synergistic improvement of the "mechanical-electrical" performance of the insulating rods.
[0004] To achieve the above object, the present invention provides a method for improving the performance of an aramid insulating pull rod based on interface functional modification, which specifically comprises the following steps:
[0005] S1, introducing polar groups on the surface of aramid fibers;
[0006] S2, immersing the polar group-modified aramid fiber in an alkaline graphene oxide solution to obtain graphene oxide-modified aramid fiber;
[0007] S3, washing and drying the aramid fiber modified with graphene oxide to obtain modified aramid fiber;
[0008] S4, using modified aramid fiber to wind the insulating pull rod for GIS;
[0009] S5. The formed insulating rod is vacuum impregnated with an epoxy resin-anhydride system and subjected to high-temperature curing treatment to obtain an aramid insulating rod based on interface functionalization modification.
[0010] Preferably, the step S1 specifically includes the following steps:
[0011] S1-1, washing the aramid fiber and drying it;
[0012] S1-2, subjecting the cleaned and dried aramid fibers to plasma discharge pretreatment;
[0013] S1-3, immersing the aramid fiber pretreated by plasma discharge in a solution containing polar groups to obtain aramid fiber modified by polar groups;
[0014] S1-4, washing and drying the aramid fibers modified with polar groups.
[0015] Preferably, in step S1-2, the plasma discharge pretreatment adopts a dielectric barrier discharge form, the gas atmosphere is an argon atmosphere, and the parameters of this treatment process are: voltage 3-5 kV, frequency 20-40 kHz, treatment time 1-3 min, and flow rate 1-3 L / min.
[0016] Preferably, in step S1-3, the polar group is one of amino, hydroxyl, carboxyl and epoxy groups, and the aramid fiber is immersed in the polar group solution for 6 to 24 hours at a temperature of 25 to 60°C.
[0017] Preferably, in steps S1-3 and S3, the cleaning and drying methods are: repeatedly cleaning the modified aramid fiber with deionized water, and vacuum drying at 60° C. for 6 to 8 hours.
[0018] Preferably, in step S2, the preparation method of the alkaline graphene oxide solution is: adding graphene oxide nanoparticles to 10mM Tris-HCl buffer with a pH of 8.5, stirring and then ultrasonicating to obtain an alkaline graphene oxide solution with a graphene oxide content of 0.5 to 1.5g / L.
[0019] Preferably, in step S2, the aramid fiber is immersed in the alkaline graphene oxide solution for 8 to 12 hours at a temperature of 25 to 60°C.
[0020] Preferably, in step S5, the room temperature viscosity of the epoxy resin-anhydride system solution is less than 1000 mPa·s; the resin mixture system is poured into a product mold by vacuum pouring equipment for high-temperature curing, and the curing conditions are: maintaining at 80-100° C. for 4-12 hours, and then maintaining at 120-140° C. for 4-24 hours.
[0021] Therefore, the present invention provides a method for improving the performance of aramid insulating pull rod based on interface functional modification, and the specific beneficial effects are as follows:
[0022] The present invention firstly improves the surface activity and roughness of aramid fiber through plasma discharge pretreatment, which does not affect the intrinsic strength of the fiber and provides reaction sites for subsequent modification methods; then, a large number of polar groups are introduced on the fiber surface by using a chemical polar group solution, which enhances the chemical bonding strength between the fiber and the matrix, alleviates the interface stress concentration and reduces the formation of defects; finally, the graphene oxide is introduced as a nano-functional filler, and the large specific surface area and mechanical anchor point function brought by it are utilized to enhance the mechanical interlocking effect of the fiber / matrix interface, and at the same time, the rich surface groups and quantum well effect are utilized to increase the charge capture function at the interface and inhibit insulation degradation, thereby constructing an interface multi-scale functional layer, achieving a significant improvement in the interface bonding strength between the aramid fiber and the epoxy, and achieving a synergistic improvement in the "mechanical-electrical" performance of the insulating pull rod.
[0023] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 is a modification process flow chart of the present invention;
[0025] Figure 2 is a SEM image of the surface of the aramid fiber before and after the modification treatment of the present invention;
[0026] Figure 3 1 is an XPS graph of the aramid fiber before and after the modification treatment of the present invention;
[0027] Figure 4 It is a comparison diagram of the interface shear strength data of the insulating pull rod before and after the modification of the present invention;
[0028] Figure 5 It is a comparison chart of AC breakdown strength data of the insulating pull rod before and after modification of the present invention;
[0029] Figure 6 It is a comparison chart of DC conductivity data of the insulating pull rod before and after modification of the present invention. DETAILED DESCRIPTION
[0030] The present invention is further described below in conjunction with embodiments. The detailed description of the embodiments of the present invention provided below is not intended to limit the scope of the invention claimed for protection, but only represents selected embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Example 1
[0032] like Figure 1 As shown, this embodiment provides a method for improving the performance of an aramid insulating pull rod based on interface functional modification, which specifically includes the following steps:
[0033] Step 1: Wash the aramid fiber and dry it.
[0034] In this step, the aramid fiber is first heated and cleaned in a 100° C. deionized water bath for 4 h, then ultrasonically cleaned with anhydrous ethanol for 1 h, and finally dried in a 60° C. oven for 6 h.
[0035] Step 2: Pre-treating the cleaned and dried aramid fibers by plasma discharge.
[0036] In this step, the plasma discharge pretreatment adopts the form of dielectric barrier discharge, and the gas atmosphere is an argon atmosphere. During this treatment process, the setting parameters are: voltage 5kV, frequency 30kHz, treatment time 2min, and argon flow rate 2L / min.
[0037] Step 3: Soaking the aramid fiber pretreated by plasma discharge in an alkaline dopamine solution to obtain dopamine-modified aramid fiber.
[0038] In this step, 182 mg of tris(hydroxymethyl)aminomethane was first weighed and added to 150 mL of deionized water, followed by 50 mL of anhydrous ethanol and 400 mg of dopamine hydrochloride, stirred with a glass rod, and placed in an ultrasonic instrument at 175 W for 30 minutes to obtain an alkaline dopamine solution with a pH of 8.5 and a dopamine content of 2 g / L. After the alkaline dopamine solution was prepared, the aramid fiber treated in step 2 above was immersed in the alkaline dopamine solution for 12 hours, and the ambient temperature was set to 25°C.
[0039] Step 4: Clean and dry the dopamine-modified aramid fiber.
[0040] In this step, the treated aramid fiber is repeatedly washed with deionized water and vacuum dried at 60° C. for 6 h.
[0041] Step 5: Immerse the washed and dried aramid fibers in an alkaline graphene oxide solution to obtain graphene oxide-modified aramid fibers.
[0042] In this step, first weigh 0.2g of graphene oxide nanoparticles and add them to 200mL of 10mM Tris-HCl (trishydroxymethylaminomethane-hydrogen chloride) buffer with a pH of 8.5, stir with a glass rod and place in an ultrasonic instrument for ultrasonic treatment for 30 minutes to obtain an alkaline graphene oxide solution with a pH of 8.5 and a graphene oxide content of 1g / L. After the alkaline graphene oxide solution is prepared, the aramid fiber treated in step 4 above is immersed in the alkaline graphene oxide solution for 10h, and the ambient temperature is set to 25°C.
[0043] Step 6: Clean and dry the aramid fiber modified with graphene oxide.
[0044] In this step, the treated aramid fiber is repeatedly washed with deionized water and vacuum dried at 60° C. for 6 h.
[0045] Step 7: vacuum pressure impregnate the treated aramid fiber with epoxy resin, and perform high temperature curing and post-curing treatment to obtain an insulating pull rod with multi-scale interface modification.
[0046] In this step, the composite material after vacuum impregnation is cured at high temperature. The specific curing conditions are firstly maintained at 100° C. for 4 hours and then maintained at 120° C. for 4 hours.
[0047] like Figure 2 As shown, by comparing the SEM images of the aramid fiber before and after modification in this embodiment, it can be seen that the surface of the aramid fiber is relatively smooth before modification, and after the interface functionalization modification treatment, the surface of the aramid fiber becomes rough and uneven, and typical flaky structure attachments appear in many places.
[0048] like Figure 3 As shown, by comparing the XPS spectra of the aramid fiber before and after modification in this embodiment, it can be seen that after the interface functionalization modification treatment, the content of N element in the C1s fine spectrum of the aramid fiber is reduced, and the content of O element is increased. At the same time, it can be decomposed into peaks such as -C=C-(284.2eV), -CC-(284.8eV), -CO-(286.1eV), -COC-(286.8eV), C=O(288eV) and -COO-(290eV), which are consistent with the C1s narrow spectrum of graphene oxide. Figure 1 This further proves that graphene oxide was successfully introduced into the surface of aramid fiber.
[0049] like Figure 4As shown, the interface shear strength of the insulating rod before modification in this embodiment is 29.1 MPa, and after modification, the interface shear strength reaches 68.5 MPa. From this result, it can be concluded that after the interface functionalization modification treatment, the interface shear strength of the insulating rod is increased by 135.40%.
[0050] like Figure 5 As shown, the AC breakdown strength of the insulating rod before modification in this embodiment is 29.22 kV / mm, and after modification, the AC breakdown strength reaches 38.16 kV / mm. From this result, it can be concluded that after the interface functionalization modification treatment, the AC breakdown strength of the insulating rod is increased by 30.60%.
[0051] like Figure 6 As shown in the figure, the DC conductivity of the insulating pull rod before and after modification in this embodiment is 3.52×10 -14 S / m and 6.57×10 -15 S / m. From this result, it can be concluded that the conductivity of the insulating rod is reduced by 81.31% after the interface functionalization modification treatment.
[0052] In summary, the present invention provides a method for improving the performance of aramid insulating rods based on interface functional modification, in which the surface activity and roughness of aramid fibers are improved by plasma discharge pretreatment, and then a large number of amino polar groups are introduced on the fiber surface by dopamine coating treatment. Finally, nano-graphene oxide is used to give the interface mechanical anchor points and charge capture functions, thereby constructing a multi-scale functional layer of the interface, thereby achieving a synergistic improvement in the "mechanical-electrical" performance of the insulating rod.
[0053] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for improving the performance of aramid insulating pull rod based on interface functional modification, characterized in that: The specific steps include: S1, introducing polar groups on the surface of aramid fibers; S2, immersing the polar group-modified aramid fiber in an alkaline graphene oxide solution to obtain graphene oxide-modified aramid fiber; S3, washing and drying the aramid fiber modified with graphene oxide to obtain modified aramid fiber; S4, using modified aramid fiber to wind the insulating pull rod for GIS; S5, vacuum impregnating the formed insulating rod with an epoxy resin-anhydride system, and performing high-temperature curing treatment to obtain an aramid insulating rod based on interface functionalization modification; In step S2, the preparation method of the alkaline graphene oxide solution is: adding graphene oxide nanoparticles into 10mM Tris-HCl buffer with a pH of 8.5, stirring and then ultrasonicating to obtain an alkaline graphene oxide solution with a graphene oxide content of 0.5 to 1.5g / L.
2. The method for improving the performance of aramid insulating pull rod based on interface functional modification according to claim 1, characterized in that: The step S1 specifically includes the following steps: S1-1, washing the aramid fiber and drying it; S1-2, subjecting the cleaned and dried aramid fibers to plasma discharge pretreatment; S1-3, immersing the aramid fiber pretreated by plasma discharge in a solution containing polar groups to obtain aramid fiber modified by polar groups; S1-4, washing and drying the aramid fibers modified with polar groups.
3. The method for improving the performance of aramid insulating pull rod based on interface functional modification according to claim 2, characterized in that: In step S1-2, the plasma discharge pretreatment adopts the dielectric barrier discharge form, the gas atmosphere is an argon atmosphere, and the parameters of this treatment process are: voltage 3-5kV, frequency 20-40kHz, treatment time 1-3min, flow rate 1-3L / min.
4. The method for improving the performance of aramid insulating pull rod based on interface functional modification according to claim 2, characterized in that: In step S1-3, the polar group is one of amino, hydroxyl, carboxyl and epoxy groups, and the aramid fiber is immersed in the polar group solution for 6 to 24 hours at a temperature of 25 to 60°C.
5. The method for improving the performance of aramid insulating pull rod based on interface functional modification according to claim 2, characterized in that: In the steps S1-3 and S3, the cleaning and drying methods are: repeatedly cleaning the modified aramid fiber with deionized water, and vacuum drying at 60° C. for 6 to 8 hours.
6. The method for improving the performance of aramid insulating pull rod based on interface functional modification according to claim 1, characterized in that: In step S2, the aramid fiber is immersed in the alkaline graphene oxide solution for 8 to 12 hours at a temperature of 25 to 60°C.
7. The method for improving the performance of aramid insulating pull rod based on interface functional modification according to claim 1, characterized in that: In the step S5, the room temperature viscosity of the epoxy resin-anhydride system solution is less than 1000 mPa·s; the resin mixture system is poured into a product mold by vacuum pouring equipment for high-temperature curing, and the curing conditions are: maintaining at 80-100° C. for 4-12 hours, and then maintaining at 120-140° C. for 4-24 hours.