A high weather-resistant and high-corrosion-resistant powder coating for energy storage equipment and a preparation method thereof

By using powder coatings of modified nano-alumina, modified nano-titanium dioxide and other materials in energy storage equipment, combined with specific processes and additives, the deficiencies in weather resistance and corrosion resistance of solid coatings in energy storage equipment are solved. solve the problem and achieve high weather resistance and high corrosion resistance coating, reducing environmental pollution.

CN118546587BActive Publication Date: 2024-10-29FOSHAN TUYI DECORATIVE MATERIAL TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411016782.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-29
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

Existing solid coatings have poor weather resistance and corrosion resistance in energy storage equipment, and traditional coatings release volatile harmful gases during the curing process, causing environmental pollution.

Method used

Use powder coatings composed of modified nano-alumina, modified nano-titanium dioxide, methyl etherified melamine resin, etc., through specific modification processes and additives to improve the weather resistance and corrosion resistance of the coating, including modified nano The preparation method of alumina and the addition of talc modifier, the preparation method of modified nano-titanium dioxide and the use of silane coupling agent.

Benefits of technology

It significantly improves the weather resistance and corrosion resistance of powder coatings, reduces environmental pollution, is suitable for energy storage equipment, and has broad market application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention belongs to the technical field of coatings, and specifically relates to a powder coating with high weather resistance and high corrosion resistance for energy storage equipment and a preparation method thereof, comprising the following components in mass percentage: 2-6wt% pigment, 25-33wt% modified nano titanium dioxide, 20-28% modified nano aluminum oxide, 2-4% defoamer, 4-7% anti-settling agent, 1-2% organic matting agent, and the balance is methyl etherified melamine resin. The present invention is compounded by resin and a variety of modified solid powders, and a variety of additives are added, and the compatibility of each component in the system is high, the obtained powder coating has good weather resistance and high corrosion resistance, is suitable for use as a coating for energy storage equipment, and has broad market value and application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of coatings, and in particular relates to a powder coating with high weather resistance and high corrosion resistance for energy storage equipment and a preparation method thereof. Background Art

[0002] Energy storage equipment mainly refers to various devices used to store energy. These devices play an important role in power systems, portable electronic devices, transportation, and renewable energy. Common energy storage devices include batteries (such as lithium-ion batteries, lead-acid batteries, sodium-sulfur batteries, etc.), supercapacitors, flywheel energy storage, pumped storage, and compressed air energy storage. Each energy storage technology has its own unique advantages and disadvantages and is suitable for different application scenarios.

[0003] The application of coatings in energy storage devices is mainly to improve performance, safety and durability. The coating should be able to enhance the mechanical strength of the energy storage device shell and resist physical damage such as impact and wear. With the increasing requirements for sustainable development, the development of low-VOC (volatile organic compounds) or even VOC-free environmentally friendly coatings has become a trend. Powder coatings, because they rarely release volatile harmful gases into the environment during coating and curing, and do not cause environmental problems such as air pollution, their application areas are constantly expanding. However, the weather resistance and corrosion resistance of solid coatings currently on the market are not good. Summary of the invention

[0004] The purpose of the present invention is to provide a powder coating with high weather resistance and high corrosion resistance for energy storage equipment and a preparation method thereof.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] A highly weather-resistant and corrosion-resistant powder coating for energy storage equipment comprises the following components in percentage by mass: 2-6wt% pigment, 25-33wt% modified nano titanium dioxide, 20-28% modified nano aluminum oxide, 2-4% defoaming agent, 4-7% anti-settling agent, 1-2% organic matting agent, and the balance is methyl etherified melamine resin.

[0007] The inventors of the present invention have found that if one of modified nano-alumina and modified nano-titanium dioxide is not added to the product, the performance of the product will deteriorate significantly. By combining the two and working together, the product performance is most significant.

[0008] Furthermore, the preparation method of the modified nano-alumina is:

[0009] (1) calcining 10 parts by mass of nano-alumina having a particle size of 100-200 nm at 400-500° C. for 30-50 min to obtain calcined nano-alumina;

[0010] (2) adding 40-45 parts by weight of a 30-35 wt% sulfuric acid aqueous solution to the calcined nano-alumina, ultrasonicating for 30-40 min, drying, grinding, and passing through a 100 mesh sieve to obtain porous nano-alumina;

[0011] (3) Mix 1 part by mass of porous nano-alumina, 10-13 parts by mass of ethanol, 0.06-0.08 parts by mass of silane coupling agent KH550, 0.04-0.06 parts by mass of titanate coupling agent LD-4 and 0.01-0.03 parts by mass of talc modifier, stir evenly, heat to 45-50° C., stir for 2-3 hours, filter and dry to obtain modified nano-alumina;

[0012] The preparation method of the talcum powder modifier is:

[0013] The talcum powder is first immersed in a sufficient amount of yttrium nitrate solution with a mass fraction of 5% for immersion treatment, the immersion power is 350W, the immersion time is 20 minutes, and then the immersion is completed, and then filtered and dried. 4-7 weight parts of dried talcum powder, 1-3 weight parts of hydroxyapatite, 2-5 weight parts of chitosan solution, 2-4 weight parts of urea and 1-2 weight parts of lanthanum chloride solution are mixed and ball milled at a ball milling speed of 1500-2000r / min for 2h. After the ball milling is completed, the mixture is washed with water and dried to obtain a talcum powder modifier; the mass fraction of the chitosan solution is 2-5%; the mass fraction of the lanthanum chloride solution is 4-6%.

[0014] The inventors of the present invention also found that when no talc modifier was added to the modified nano alumina, the dry talc in the talc modifier was directly replaced by talc raw material, and hydroxyapatite and lanthanum chloride solution were not added to the talc modifier, the performance of the product tended to deteriorate. Only when the talc modifier obtained by the method of the present invention was added to the modified nano alumina, the product performance effect was the most significant. The effects of other methods were not as obvious as those of the present invention.

[0015] Furthermore, the preparation method of the modified nano titanium dioxide is:

[0016] (1) Under a nitrogen atmosphere, 3-pentadecylphenol, silane coupling agent KH560 and dibutyltin dilaurate in a weight ratio of 2.5-3.4:1:0.05-0.06 are mixed, heated to 80-85°C and stirred for 3-4 hours, and then a regulator in an amount of 2-5% of the total amount of the silane coupling agent KH560 is added, and stirring is continued for 1 hour to obtain a modified silane coupling agent;

[0017] The preparation method of the regulator is as follows:

[0018] 3-5 parts by weight of nano-bentonite powder, 1-2 parts by weight of stearic acid, 4-7 parts by weight of 6% sodium citrate solution and 2-4 parts by weight of nano-silica sol are mixed and ball-milled at a ball-milling speed of 1000 r / min for 2 hours. After the ball-milling is completed, the mixture is washed with water and dried to obtain a conditioning agent;

[0019] (2) Mix nano-titanium dioxide, 60-65wt% ethanol aqueous solution and modified silane coupling agent in a mass ratio of 1:10-12:0.04-0.06, stir and react at 55-60°C for 1-3h, filter, wash and dry to obtain modified nano-titanium dioxide.

[0020] Furthermore, the particle size of the nano titanium dioxide is 20-100 nm, and the average specific surface area is 235 m 2 / g.

[0021] Furthermore, the defoaming agent is an acrylic defoaming agent.

[0022] Furthermore, the anti-settling agent is gas-phase nano titanium dioxide.

[0023] Furthermore, the organic matting agent is pure polyester matting resin RB608.

[0024] Furthermore, the molecular weight of the methyl etherified melamine resin is 10000-40000, and the hydroxyl value is 50-60 mgKOH / g.

[0025] Furthermore, the solid content of the methyl etherified melamine resin is ≥ 60wt%.

[0026] Titanate coupling agent LD-4, Yangzhou Lida Resin Co., Ltd.

[0027] The invention provides a method for preparing a powder coating with high weather resistance and high corrosion resistance for energy storage equipment. The method comprises the following steps: mixing a pigment, modified nano titanium dioxide, modified nano aluminum oxide, a defoamer, an anti-settling agent, an organic matting agent and a methylated melamine resin, stirring at 2000-4000 rpm for 10 minutes, stirring at 600-800 rpm for 10 minutes, mixing evenly, kneading and extruding at 110-120° C., crushing, sieving, and controlling the particle size to be 100-200 meshes, so as to obtain a powder coating with high weather resistance and high corrosion resistance for energy storage equipment.

[0028] Compared with the prior art, the advantages and beneficial effects of the present invention are as follows: the present invention compounds resin and a variety of modified solid powders and adds a variety of additives, so that the compatibility of the components in the system is high, and the prepared powder coating has good weather resistance and high corrosion resistance, and is suitable for use as a coating for energy storage devices, and has broad market value and application prospects;

[0029] The modified nano-alumina is modified by the specific process of the present invention, and the talc modifier is added as a coordinated raw material. The talc is immersed in an yttrium nitrate solution for improvement to obtain a yttrium-doped talc agent. The yttrium-doped talc agent is coordinated with hydroxyapatite, chitosan solution, urea and lanthanum chloride solution. The raw materials are coordinated and cooperated to achieve synergistic effects. The obtained talc modifier enhances the modification effect of the modified nano-alumina in the product system, thereby improving the weather resistance and corrosion resistance of the product. To further enhance the performance, modified silane coupling agent is used for coordinated improvement in the modification of modified nano titanium dioxide. At the same time, the regulator is used as a synergistic enhancer in the improvement of modified silane coupling agent. The regulator is made of nano bentonite powder, stearic acid, 6% sodium citrate solution and nano silica sol blended and ball-milled. Lamellar bentonite is used as an interlaced reinforcing agent, and the raw materials in the regulator are used to reinforce and enhance the performance together, so that the performance of the nano titanium dioxide product modified by the modified silane coupling agent is further enhanced. DETAILED DESCRIPTION

[0030] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Example 1

[0032] The present embodiment provides a powder coating with high weather resistance and high corrosion resistance for energy storage equipment, comprising the following components in percentage by mass: 4wt% pigment, 29wt% modified nano titanium dioxide, 25% modified nano aluminum oxide, 3% defoaming agent, 5% anti-settling agent, 1.6% organic matting agent, and the balance is methyl etherified melamine resin.

[0033] The preparation method of the modified nano alumina is:

[0034] (1) calcining 10 parts by mass of nano-alumina having a particle size of 100-200 nm at 450° C. for 40 minutes to obtain calcined nano-alumina;

[0035] (2) adding 42 parts by mass of a 32 wt% sulfuric acid aqueous solution to the calcined nano-alumina, ultrasonicating for 35 min, drying, grinding, and passing through a 100-mesh sieve to obtain porous nano-alumina;

[0036] (3) Mix 1 part by mass of porous nano-alumina, 12 parts by mass of ethanol, 0.07 parts by mass of silane coupling agent KH550, 0.05 parts by mass of titanate coupling agent LD-4 and 0.02 parts by mass of talcum powder modifier, stir evenly, heat to 48°C, stir for 2.4 hours, filter and dry to obtain modified nano-alumina.

[0037] The preparation method of the talcum powder modifier is:

[0038] The talcum powder is first immersed in a sufficient amount of yttrium nitrate solution with a mass fraction of 5% for immersion treatment, the immersion power is 350W, the immersion time is 20min, and then the immersion is completed, and then filtered and dried. 5.5 parts by weight of dry talcum powder, 2 parts by weight of hydroxyapatite, 3.5 parts by weight of chitosan solution, 3 parts by weight of urea and 1.5 parts by weight of lanthanum chloride solution are mixed and ball milled at a ball milling speed of 1700r / min for 2h. After the ball milling is completed, the mixture is washed with water and dried to obtain a talcum powder modifier; the mass fraction of the chitosan solution is 3.5%; the mass fraction of the lanthanum chloride solution is 5%.

[0039] The preparation method of the modified nano titanium dioxide is:

[0040] (1) Under a nitrogen atmosphere, 3-pentadecylphenol, silane coupling agent KH560 and dibutyltin dilaurate in a weight ratio of 3:1:0.06 were mixed, heated to 82°C and stirred for 3.4 hours, and then a regulator in an amount of 3.5% of the total amount of silane coupling agent KH560 was added, and stirring was continued for 1 hour to obtain a modified silane coupling agent;

[0041] The preparation method of the regulator is as follows:

[0042] 4 parts by weight of nano-bentonite powder, 1.5 parts by weight of stearic acid, 5.5 parts by weight of 6% sodium citrate solution and 3 parts by weight of nano-silica sol were mixed and ball-milled at a ball-milling speed of 1000 r / min for 2 h. After the ball-milling was completed, the mixture was washed with water and dried to obtain a conditioning agent;

[0043] (2) Mix nano-titanium dioxide, 62 wt% ethanol aqueous solution and modified silane coupling agent in a mass ratio of 1:11:0.05, stir and react at 57°C for 2 h, filter, wash and dry to obtain modified nano-titanium dioxide.

[0044] The particle size of the nano titanium dioxide is 50nm and the average specific surface area is 235m 2 / g.

[0045] The defoamer is an acrylic defoamer.

[0046] The anti-settling agent is gas-phase nano titanium dioxide.

[0047] The organic matting agent is pure polyester matting resin RB608.

[0048] The molecular weight of the methyl etherified melamine resin is 20000, the hydroxyl value is 50 mgKOH / g, and the solid content of the methyl etherified melamine resin is ≥ 60 wt%.

[0049] Titanate coupling agent LD-4, Yangzhou Lida Resin Co., Ltd.

[0050] The preparation method of the highly weather-resistant and highly corrosion-resistant powder coating for energy storage equipment comprises the following steps: mixing pigment, modified nano titanium dioxide, modified nano aluminum oxide, defoamer, anti-settling agent, organic matting agent and methyl etherified melamine resin, stirring at 3000 rpm for 10 minutes, stirring at 700 rpm for 10 minutes, mixing evenly, kneading and extruding at 115° C., crushing and sieving, and controlling the particle size to be 100-200 meshes to obtain the highly weather-resistant and highly corrosion-resistant powder coating for energy storage equipment.

[0051] Example 2

[0052] The present embodiment provides a powder coating with high weather resistance and high corrosion resistance for energy storage equipment, comprising the following components in percentage by mass: 6wt% pigment, 25wt% modified nano titanium dioxide, 28% modified nano aluminum oxide, 2% defoaming agent, 7% anti-settling agent, 1% organic matting agent, and the balance is methyl etherified melamine resin.

[0053] The preparation method of the modified nano alumina is:

[0054] (1) calcining 10 parts by mass of nano-alumina having a particle size of 100-200 nm at 500° C. for 30 minutes to obtain calcined nano-alumina;

[0055] (2) adding 45 parts by mass of a 30 wt% sulfuric acid aqueous solution to the calcined nano-alumina, ultrasonicating for 40 min, drying, grinding, and passing through a 100-mesh sieve to obtain porous nano-alumina;

[0056] (3) Mix 1 part by mass of porous nano-alumina, 10 parts by mass of ethanol, 0.08 parts by mass of silane coupling agent KH550, 0.04 parts by mass of titanate coupling agent LD-4 and 0.03 parts by mass of talcum powder modifier, stir evenly, heat to 45°C, stir for 3 hours, filter and dry to obtain modified nano-alumina.

[0057] The preparation method of the talcum powder modifier is:

[0058] The talcum powder is first immersed in a sufficient amount of yttrium nitrate solution with a mass fraction of 5% for immersion treatment, the immersion power is 350W, the immersion time is 20min, and then the immersion is completed, and then filtered and dried. 4 parts by weight of dry talcum powder, 3 parts by weight of hydroxyapatite, 2 parts by weight of chitosan solution, 4 parts by weight of urea and 1 part by weight of lanthanum chloride solution are mixed and ball milled at a ball milling speed of 2000r / min for 2h. After the ball milling is completed, the mixture is washed with water and dried to obtain a talcum powder modifier; the mass fraction of the chitosan solution is 2%; the mass fraction of the lanthanum chloride solution is 6%.

[0059] The preparation method of the modified nano titanium dioxide is:

[0060] (1) Under a nitrogen atmosphere, 3-pentadecylphenol, silane coupling agent KH560 and dibutyltin dilaurate in a weight ratio of 2.5:1:0.06 were mixed, heated to 80-85°C and stirred for 3 hours, and then a regulator of 2% of the total amount of silane coupling agent KH560 was added, and stirring was continued for 1 hour to obtain a modified silane coupling agent;

[0061] The preparation method of the regulator is as follows:

[0062] 3 parts by weight of nano-bentonite powder, 2 parts by weight of stearic acid, 4 parts by weight of 6% sodium citrate solution and 2 parts by weight of nano-silica sol are mixed and ball-milled at a ball-milling speed of 1000 r / min for 2 h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a conditioning agent;

[0063] (2) Mix nano-titanium dioxide, 60 wt% ethanol aqueous solution and modified silane coupling agent in a mass ratio of 1:10:0.06, stir and react at 60°C for 1 hour, filter, wash and dry to obtain modified nano-titanium dioxide.

[0064] The particle size of the nano titanium dioxide is 20-100nm, and the average specific surface area is 235m 2 / g.

[0065] The defoamer is an acrylic defoamer.

[0066] The anti-settling agent is gas-phase nano titanium dioxide.

[0067] The organic matting agent is pure polyester matting resin RB608.

[0068] The molecular weight of the methyl etherified melamine resin is 10,000, and the hydroxyl value is 50 mgKOH / g.

[0069] The solid content of the methyl etherified melamine resin is ≥60wt%.

[0070] Titanate coupling agent LD-4, Yangzhou Lida Resin Co., Ltd.

[0071] The preparation method of the highly weather-resistant and highly corrosion-resistant powder coating for energy storage equipment comprises the following steps: mixing pigment, modified nano titanium dioxide, modified nano aluminum oxide, defoamer, anti-settling agent, organic matting agent and methyl etherified melamine resin, stirring at 4000 rpm for 10 minutes, stirring at 600 rpm for 10 minutes, mixing evenly, kneading and extruding at 120° C., crushing and sieving, and controlling the particle size to 100 meshes to obtain the highly weather-resistant and highly corrosion-resistant powder coating for energy storage equipment.

[0072] Example 3

[0073] The present embodiment provides a powder coating with high weather resistance and high corrosion resistance for energy storage equipment, comprising the following components in percentage by mass: 2wt% pigment, 33wt% modified nano titanium dioxide, 20% modified nano aluminum oxide, 4% defoaming agent, 4% anti-settling agent, 2% organic matting agent, and the balance is methyl etherified melamine resin.

[0074] The preparation method of the modified nano alumina is:

[0075] (1) calcining 10 parts by weight of nano-alumina having a particle size of 200 nm at 400° C. for 50 min to obtain calcined nano-alumina;

[0076] (2) adding 40 parts by weight of a 35 wt% sulfuric acid aqueous solution to the calcined nano-alumina, ultrasonicating for 30 min, drying, grinding, and passing through a 100-mesh sieve to obtain porous nano-alumina;

[0077] (3) Mix 1 part by mass of porous nano-alumina, 13 parts by mass of ethanol, 0.06 parts by mass of silane coupling agent KH550, 0.06 parts by mass of titanate coupling agent LD-4 and 0.01 parts by mass of talcum powder modifier, stir evenly, heat to 50° C., stir for 2 h, filter and dry to obtain modified nano-alumina.

[0078] The preparation method of the talcum powder modifier is:

[0079] The talcum powder is first immersed in a sufficient amount of yttrium nitrate solution with a mass fraction of 5% for immersion treatment, the immersion power is 350W, the immersion time is 20min, and then the immersion is completed, and then filtered and dried. 7 parts by weight of dry talcum powder, 3 parts by weight of hydroxyapatite, 2 parts by weight of chitosan solution, 2 parts by weight of urea and 1 part by weight of lanthanum chloride solution are mixed and ball milled at a ball milling speed of 1500r / min for 2h. After the ball milling is completed, the mixture is washed with water and dried to obtain a talcum powder modifier; the mass fraction of the chitosan solution is 5%; the mass fraction of the lanthanum chloride solution is 6%.

[0080] The preparation method of the modified nano titanium dioxide is:

[0081] (1) Under a nitrogen atmosphere, 3-pentadecylphenol, silane coupling agent KH560 and dibutyltin dilaurate in a weight ratio of 3.4:1:0.05 were mixed, heated to 85°C and stirred for 3 hours, and then a regulator in an amount of 2% of the total amount of the silane coupling agent KH560 was added, and stirring was continued for 1 hour to obtain a modified silane coupling agent;

[0082] The preparation method of the regulator is as follows:

[0083] 5 parts by weight of nano-bentonite powder, 1 part by weight of stearic acid, 7 parts by weight of 6% sodium citrate solution and 4 parts by weight of nano-silica sol are mixed and ball-milled at a ball-milling speed of 1000 r / min for 2 hours. After the ball-milling is completed, the mixture is washed with water and dried to obtain a conditioning agent;

[0084] (2) Mix nano-titanium dioxide, 65 wt% ethanol aqueous solution and modified silane coupling agent in a mass ratio of 1:12:0.04, stir and react at 55°C for 3 hours, filter, wash and dry to obtain modified nano-titanium dioxide.

[0085] The particle size of the nano titanium dioxide is 100 nm, and the average specific surface area is 235 m 2 / g.

[0086] The defoamer is an acrylic defoamer.

[0087] The anti-settling agent is gas-phase nano titanium dioxide.

[0088] The organic matting agent is pure polyester matting resin RB608.

[0089] The molecular weight of methyl etherified melamine resin is 40,000 and the hydroxyl value is 50 mgKOH / g.

[0090] The solid content of the methyl etherified melamine resin is ≥60wt%.

[0091] Titanate coupling agent LD-4, Yangzhou Lida Resin Co., Ltd.

[0092] The preparation method of the highly weather-resistant and highly corrosion-resistant powder coating for energy storage equipment comprises the following steps: mixing pigment, modified nano titanium dioxide, modified nano aluminum oxide, defoamer, anti-settling agent, organic matting agent and methyl etherified melamine resin, stirring at 2000 rpm for 10 minutes, stirring at 800 rpm for 10 minutes, mixing evenly, kneading and extruding at 110° C., crushing and sieving, and controlling the particle size to be 100-200 meshes, so as to obtain the highly weather-resistant and highly corrosion-resistant powder coating for energy storage equipment.

[0093] Comparative Example 1

[0094] The difference between this comparative example and Example 1 is that the composition ratio is different.

[0095] A highly weather-resistant and corrosion-resistant powder coating for energy storage equipment comprises the following components in percentage by mass: 4wt% pigment, 20wt% modified nano titanium dioxide, 34% modified nano aluminum oxide, 3% defoaming agent, 5% anti-settling agent, 1.6% organic matting agent, and the balance is methyl etherified melamine resin.

[0096] Comparative Example 2

[0097] The difference between this comparative example and Example 1 is that the composition ratio is different.

[0098] A highly weather-resistant and corrosion-resistant powder coating for energy storage equipment comprises the following components in percentage by mass: 4wt% pigment, 39wt% modified nano titanium dioxide, 15% modified nano aluminum oxide, 3% defoaming agent, 5% anti-settling agent, 1.6% organic matting agent, and the balance is methyl etherified melamine resin.

[0099] Comparative Example 3

[0100] The difference between this comparative example and Example 1 is that no modified nano titanium dioxide is added.

[0101] Comparative Example 4

[0102] The difference between this comparative example and Example 1 is that the modified silane coupling agent in the preparation of modified nano-titanium dioxide is replaced by silane coupling agent KH560.

[0103] Comparative Example 5

[0104] The difference between this comparative example and Example 1 is that no regulator is added in the preparation of the modified nano titanium dioxide.

[0105] Comparative Example 6

[0106] The difference between this comparative example and Example 1 is that the preparation method of the regulator is different. 5 parts of nano-bentonite powder and 7 parts of 6% sodium citrate solution are blended and ball-milled at a ball-milling speed of 1000 r / min for 2 hours. After the ball-milling is completed, the mixture is washed with water and dried to obtain the regulator.

[0107] Comparative Example 7

[0108] The difference between this comparative example and Example 1 is that no modified nano-alumina is added.

[0109] Comparative Example 8

[0110] The difference between this comparative example and Example 1 is that no talcum powder modifier is added to the modified nano-alumina.

[0111] Comparative Example 9

[0112] The difference between this comparative example and Example 1 is that the dry talc in the talc modifier is directly replaced by talc raw material.

[0113] Comparative Example 10

[0114] The difference between this comparative example and Example 1 is that no hydroxyapatite or lanthanum chloride solution is added to the talc modifier.

[0115] Performance Testing

[0116] The solid coatings of Examples 1-3 and Comparative Examples 1-10 were cured at a PMT metal plate temperature of 232±5° C., with a dry coating film thickness of 20 μm, and performance tests were performed. The results are shown in Table 1.

[0117] 1. MEK (methyl ethyl ketone) resistance: Tested in accordance with GB / T 13448-2019.

[0118] 2. QUVA test (1500h): Tested in accordance with ASTM D-3794.

[0119] 3. Salt spray test (1500h): Test in accordance with GB / T10125-2021.

[0120] Table 1 Performance test results

[0121]

[0122] The results show that the solid coatings prepared in Examples 1-3 of the present invention have good weather resistance and corrosion resistance. Comparative Examples 1-10 show that the comprehensive performance decreases when the preparation conditions are changed. Examples 1-3 of the present invention compound the resin and a variety of modified solid powders and add a variety of additives. The compatibility of the components in the system is high, and the powder coatings prepared have good weather resistance and high corrosion resistance. They are suitable for use as coatings for energy storage devices and have broad market value and application prospects.

[0123] If modified nano-alumina or modified nano-titanium dioxide is not added to the product, the performance of the product will be significantly deteriorated. The synergistic effect of the two is used to achieve the most significant product performance.

[0124] The performance of the products tended to deteriorate when no talc modifier was added to the modified nano-alumina, the dried talc in the talc modifier was directly replaced by talc raw material, and hydroxyapatite and lanthanum chloride solution were not added to the talc modifier. Only when the talc modifier obtained by the method of the present invention was added to the modified nano-alumina, the product performance effect was the most significant. The effects of other methods were not as obvious as those of the present invention.

[0125] In the preparation of modified nano titanium dioxide, the modified silane coupling agent is replaced by silane coupling agent KH560, no regulator is added in the preparation of modified nano titanium dioxide, and the preparation methods of the regulator are different. The performance of the product tends to deteriorate. Only when the modified nano titanium dioxide is obtained by the method of the present invention, the performance effect of the product is the most significant.

[0126] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A powder coating with high weather resistance and high corrosion resistance for energy storage equipment, characterized in that: The invention comprises the following components in percentage by weight: 2-6 wt% of pigment, 25-33 wt% of modified nano titanium dioxide, 20-28% of modified nano aluminum oxide, 2-4% of defoaming agent, 4-7% of anti-settling agent, 1-2% of organic matting agent, and the balance is methyl etherified melamine resin; The preparation method of the modified nano alumina is: (1) calcining 10 parts by mass of nano-alumina having a particle size of 100-200 nm at 400-500° C. for 30-50 min to obtain calcined nano-alumina; (2) adding 40-45 parts by weight of a 30-35 wt% sulfuric acid aqueous solution to the calcined nano-alumina, ultrasonicating for 30-40 min, drying, grinding, and passing through a 100 mesh sieve to obtain porous nano-alumina; (3) Mix 1 part by mass of porous nano-alumina, 10-13 parts by mass of ethanol, 0.06-0.08 parts by mass of silane coupling agent KH550, 0.04-0.06 parts by mass of titanate coupling agent LD-4 and 0.01-0.03 parts by mass of talc modifier, stir evenly, heat to 45-50° C., stir for 2-3 hours, filter and dry to obtain modified nano-alumina; The preparation method of the modified nano titanium dioxide is: (1) Under a nitrogen atmosphere, 3-pentadecylphenol, silane coupling agent KH560 and dibutyltin dilaurate in a weight ratio of 2.5-3.4:1:0.05-0.06 are mixed, heated to 80-85°C and stirred for 3-4 hours, and then a regulator in an amount of 2-5% of the total amount of the silane coupling agent KH560 is added, and stirring is continued for 1 hour to obtain a modified silane coupling agent; The preparation method of the regulator is as follows: 3-5 parts by weight of nano-bentonite powder, 1-2 parts by weight of stearic acid, 4-7 parts by weight of 6% sodium citrate solution and 2-4 parts by weight of nano-silica sol are mixed and ball-milled at a ball-milling speed of 1000 r / min for 2 hours. After the ball-milling is completed, the mixture is washed with water and dried to obtain a conditioning agent; (2) Mix nano titanium dioxide, 60-65wt% ethanol aqueous solution and modified silane coupling agent in a mass ratio of 1:10-12:0.04-0.06, stir at 55-60°C for 1-3h, filter, wash and dry to obtain modified nano titanium dioxide; The preparation method of the talcum powder modifier is: The talcum powder is first immersed in a sufficient amount of yttrium nitrate solution with a mass fraction of 5% for immersion treatment, the immersion power is 350W, the immersion time is 20min, and then the immersion is completed, and then filtered and dried. 4-7 weight parts of dry talcum powder, 1-3 weight parts of hydroxyapatite, 2-5 weight parts of chitosan solution, 2-4 weight parts of urea and 1-2 weight parts of lanthanum chloride solution are mixed and ball milled at a ball milling speed of 1500-2000r / min for 2h. After the ball milling is completed, the mixture is washed with water and dried to obtain a talcum powder modifier.

2. The highly weather-resistant and corrosion-resistant powder coating for energy storage equipment according to claim 1, characterized in that: The mass fraction of the chitosan solution is 2-5%; the mass fraction of the lanthanum chloride solution is 4-6%.

3. The highly weather-resistant and corrosion-resistant powder coating for energy storage equipment according to claim 2, characterized in that: The particle size of the nano titanium dioxide is 20-100nm, and the average specific surface area is 235m 2 / g.

4. The highly weather-resistant and corrosion-resistant powder coating for energy storage equipment according to claim 1, characterized in that: The defoaming agent is an acrylic defoaming agent; the anti-settling agent is gas-phase nano titanium dioxide; and the organic matting agent is pure polyester matting resin RB608.

5. The highly weather-resistant and corrosion-resistant powder coating for energy storage equipment according to claim 1, characterized in that: The molecular weight of methyl etherified melamine resin is 10000~40000, and the hydroxyl value is 50~60mgKOH / g.

6. The highly weather-resistant and corrosion-resistant powder coating for energy storage equipment according to claim 1, characterized in that: The solid content of the methyl etherified melamine resin is ≥60wt%.

7. A method for preparing a highly weather-resistant and highly corrosion-resistant powder coating for energy storage equipment according to any one of claims 1 to 6, characterized in that: The method comprises the following steps: mixing pigment, modified nano titanium dioxide, modified nano aluminum oxide, defoamer, anti-settling agent, organic matting agent and methyl etherified melamine resin, stirring at 2000-4000 rpm for 10 minutes, stirring at 600-800 rpm for 10 minutes, mixing evenly, kneading and extruding at 110-120 DEG C, crushing and sieving, and controlling the particle size to be 100-200 meshes, so as to obtain a powder coating with high weather resistance and high corrosion resistance for energy storage equipment.

Citation Information

Patent Citations

  • Nano-modified epoxy powder coating and preparation method thereof

    CN110283519A

  • Efficient anti-corrosion powder coating and preparation method thereof

    CN115386282A

  • Organic-inorganic antibacterial antifouling interior wall coating and preparation method thereof

    CN118307996A