Spherical lithium manganese iron phosphate positive electrode material and preparation method, application and lithium battery thereof

By modifying morphology, ion doping, and composite coating, spherical lithium manganese iron phosphate cathode materials were prepared, solving the problems of conductivity and structural stability of lithium manganese iron phosphate materials, improving battery performance and processing performance, and making them suitable for large-scale industrial applications.

CN118561259BActive Publication Date: 2024-11-05HUNAN YUNENG NEW ENERGY BATTERY MATERIALS CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411058153.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-05
Estimated Expiration
2044-08-02

AI Technical Summary

Technical Problem

The difference between electronic and ionic conductivity in lithium manganese iron phosphate cathode materials, the Jan Taylor effect of manganese leading to changes in crystal structure and manganese dissolution, affect their cycle performance and rate performance, and the effects of nano-sizing and carbon coating modification are limited.

Method used

By leveraging the synergistic effects of morphology control, ion doping, and composite coating with conductive carbon and fast ion conductors, spherical lithium manganese iron phosphate cathode materials were prepared. The ethylene glycol structure was used to guide the formation of self-assembled micron-sized spherical nanoparticles, which were then mixed with carbon sources and fast ion conductor lithium titanium aluminum phosphate to form a three-dimensional conductive electron and ion network.

Benefits of technology

It improves the electronic conductivity, ionic conductivity and crystal structure stability of the material, enhances the structural stability and processing performance of the material, improves the volumetric energy density and cycle life of the battery, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118561259B_ABST
    Figure CN118561259B_ABST
Patent Text Reader

Abstract

The present application belongs to the field of lithium-ion batteries, and specifically relates to a spherical lithium iron manganese phosphate positive electrode material, a preparation method thereof, an application and a lithium battery. The preparation method comprises: S1, mixing a manganese source, an iron source, a doped ion M source and a solvent to obtain a first solution; S2, mixing a phosphorus source, a lithium source and a solvent to obtain a second solution; S3, mixing the first solution and the second solution to obtain a third solution; S4, subjecting the third solution to a hydrothermal reaction, and filtering, washing and drying to obtain a first spherical lithium iron manganese phosphate positive electrode material; S5, mixing the first lithium iron manganese phosphate positive electrode material with a carbon source and a fast ion conductor lithium titanium aluminum phosphate to obtain a calcined precursor; S6, calcining the calcined precursor to obtain a second spherical lithium iron manganese phosphate positive electrode material compositely coated with carbon and a fast ion conductor, which improves the electronic conductivity, ionic conductivity and structural stability of the lithium iron manganese phosphate positive electrode material, has both high volume energy density and good processing performance, and has a simple and controllable process and low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of lithium-ion batteries, and specifically relates to spherical lithium manganese iron phosphate positive electrode materials, preparation methods, applications, and lithium batteries. Background Art

[0002] Lithium manganese iron phosphate cathode material, because it combines the high voltage advantage of lithium manganese phosphate and the excellent cycle performance of lithium iron phosphate, was once regarded as the olivine structure cathode material with the greatest market potential after lithium iron phosphate. However, due to the poor electronic conductivity and ionic conductivity of the material, the change in lattice structure induced by the Jan-Taylor effect of manganese element and the dissolution of manganese, the cycle performance and rate performance of lithium manganese iron phosphate are poor, thus hindering its commercial application process.

[0003] At present, the methods for improving the performance of lithium iron manganese phosphate materials mainly include material nano-sizing, carbon coating and ion doping. Material nano-sizing shortens the distance of ion diffusion and electron transmission, and improves the electrochemical performance of lithium iron manganese phosphate materials to a certain extent. However, material nano-sizing will reduce the volume energy density of the material, and nanomaterials are easy to agglomerate during preparation and use, and make the processing of materials difficult, which is not conducive to large-scale industrial application. Surface carbon coating can improve the electronic conductivity of lithium iron manganese phosphate positive electrode materials, but because the surface coated carbon is a loose and porous structure, it cannot effectively prevent the side reaction between the positive electrode material and the electrolyte and the dissolution of manganese ions. Ion doping can improve the intrinsic ionic conductivity and electronic conductivity of the material or stabilize the crystal structure to a certain extent, but the effect of ion doping modification alone is limited. Summary of the invention

[0004] The technical problem to be solved by this application is to overcome the deficiencies and defects mentioned in the above background technology and provide a spherical lithium manganese iron phosphate positive electrode material and its preparation method, application and lithium battery. This application combines the synergistic effect of modification methods such as morphology control, ion doping, conductive carbon and fast ion conductor composite coating, while improving the electronic conductivity, ionic conductivity and crystal structure stability of the lithium manganese iron phosphate material, improving the structural stability of the material surface, slowing down the dissolution of manganese ions, and making the material have both high volume energy density and good processing performance, with a simple preparation process and low cost, thereby obtaining a lithium ion battery positive electrode material with excellent comprehensive performance.

[0005] In order to solve the above technical problems, the technical solution proposed in this application is:

[0006] In a first aspect, the present application provides a method for preparing a spherical lithium manganese iron phosphate positive electrode material, comprising the following steps:

[0007] S1, mixing a manganese source, an iron source, a doping ion M source and a solvent to obtain a first solution;

[0008] S2, mixing a phosphorus source, a lithium source and a solvent to obtain a second solution;

[0009] S3, mixing the first solution obtained in step S1 with the second solution obtained in step S2 to obtain a third solution;

[0010] S4, subjecting the third solution to a hydrothermal reaction, and filtering, washing, and drying to obtain a first spherical lithium manganese iron phosphate positive electrode material;

[0011] S5, mixing the first spherical lithium manganese iron phosphate positive electrode material with a carbon source and a fast ion conductor lithium titanium aluminum phosphate to obtain a calcined precursor;

[0012] S6, calcining the calcined precursor to obtain a second spherical lithium manganese iron phosphate positive electrode material compositely coated with carbon and a fast ion conductor;

[0013] The solvent is ethylene glycol.

[0014] In one embodiment, the manganese source includes any one or more combinations of manganese sulfate, manganese nitrate, manganese carbonate, manganese acetate and manganese oxalate; the iron source includes any one or more combinations of iron sulfate, iron nitrate, iron acetate, iron citrate and iron oxalate;

[0015] The doping ion M source includes any one or more combinations of sulfate, nitrate, acetate, oxalate, and citrate, and the sulfate, nitrate, acetate, oxalate, and citrate all include Mg, Cu, Ni, Co, Zn, Ca, Y, Al, Ga, Zr, Ti, Cr, Mo, W, Nb, or V elements.

[0016] In one embodiment, the phosphorus source includes any one or more combinations of phosphoric acid, ammonium dihydrogen phosphate and diammonium hydrogen phosphate;

[0017] The lithium source includes any one or more combinations of lithium hydroxide, lithium nitrate, lithium carbonate, lithium dihydrogen phosphate and lithium phosphate.

[0018] In one embodiment, the temperature of the hydrothermal reaction in S4 is 200°C~250°C, the reaction time is 9 h~24 h, and the volume ratio of water to ethylene glycol in the hydrothermal reaction system is 1:(0.1-10); the molar ratio of the elements Li:Mn:Fe:P:M in the first spherical manganese iron phosphate lithium positive electrode material is (0.9~1.1):(0.1~0.9):(0.1~0.9):1:(0~0.1), and the D50 particle size of the first spherical manganese iron phosphate lithium positive electrode material is 1 μm~5 μm.

[0019] In one embodiment, the carbon source is any one or more of sucrose, glucose, fructose, polyethylene glycol, starch, citric acid, ascorbic acid, conductive carbon black, graphene, carbon nanotubes and asphalt;

[0020] The D50 particle size of the fast ion conductor lithium aluminum titanium phosphate is 0.05 μm to 1 μm.

[0021] In one embodiment, the content of conductive carbon in the second spherical lithium manganese iron phosphate positive electrode material is 1 wt% to 10 wt%;

[0022] The content of the lithium aluminum titanium phosphate is 0.1 wt% to 5 wt%.

[0023] In one embodiment, the calcination parameters in S6 are: calcination temperature is 600°C~800°C, calcination time is 2 h~12 h, and the inert gas in the calcination atmosphere is a combination of one or more of nitrogen, argon, helium, neon, krypton or xenon.

[0024] In a second aspect, the present application further provides a spherical lithium manganese iron phosphate positive electrode material prepared by the preparation method of the spherical lithium manganese iron phosphate positive electrode material as described in any one of the contents of the first aspect.

[0025] In a third aspect, the present application also provides an application of the spherical lithium manganese iron phosphate positive electrode material as described in the second aspect, for preparing a positive electrode sheet.

[0026] In a fourth aspect, the present application further provides a lithium battery, wherein the lithium-ion battery comprises a positive electrode plate as described in the third aspect.

[0027] Compared with the prior art, the beneficial effects of this application are:

[0028] (1) Through the structural guidance of ethylene glycol, the morphology is controlled under high temperature and high pressure conditions to form a micron-sized spherical lithium iron manganese phosphate positive electrode material formed by self-assembly of nanoparticles. The spherical structure is beneficial to shortening the distance of ion diffusion and electron transmission and reducing the interface resistance. The micron-sized spherical lithium iron manganese phosphate material has a stable structure, high compaction density, and relatively uniform particle size distribution, which helps to reduce the internal heterogeneity of the battery and improve the overall performance of the battery, thereby increasing the volume energy density of the lithium iron manganese phosphate battery and improving the processing performance of the material.

[0029] (2) Ion doping can effectively stabilize the crystal structure, broaden the lithium ion diffusion channel, improve the intrinsic electronic conductivity and ionic conductivity of the material, and accelerate the reaction kinetics.

[0030] (3) By calcining the precursor formed by mixing the first spherical lithium iron manganese phosphate positive electrode material with the carbon source and the fast ion conductor lithium aluminum titanium phosphate, the carbon source and the fast ion conductor material are allowed to enter the internal voids of the spherical structure to form a three-dimensional network structure of electrons and ions, thereby further improving the electronic conductivity and ionic conductivity of the lithium iron manganese phosphate positive electrode material; as an external coating layer, the composite coating process combines the high electronic conductivity of the conductive carbon and the ionic conductivity of the fast ion conductor, which can significantly improve the overall conductivity of the positive electrode material. The addition of the conductive carbon provides a fast channel for the transmission of electrons in the material, while the fast ion conductor accelerates the diffusion of lithium ions. The synergistic effect of the two improves the reaction rate and efficiency of the battery. The composite coating layer can better protect the active particles of the positive electrode material, preventing them from direct contact with the electrolyte and side reactions. The coating layer formed by the conductive carbon and the fast ion conductor can provide a more stable interface environment, reduce the generation and accumulation of harmful substances, and thus extend the cycle life of the battery. The composite coating layer can also inhibit the volume change of the positive electrode material during the charge and discharge process to a certain extent, reduce the pulverization and shedding of the material. This enhanced structural stability helps to maintain the stability and reliability of the battery. In addition, the composite coating layer formed by the carbon and fast ion conductor can effectively isolate the electrode material from direct contact with the electrolyte, avoid side reactions, and slow down the dissolution of manganese ions, thereby making the material structure more stable.

[0031] (4) This application improves the electrochemical properties and processing performance of the material through the synergistic effect of modification methods such as morphology control, ion doping, and composite coating of conductive carbon and fast ion conductors. The process is simple and controllable, with low energy consumption and cost, and is suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0033] Figure 1 A schematic flow chart of a method for preparing a spherical lithium manganese iron phosphate positive electrode material provided in one embodiment of the present application;

[0034] Figure 2 This is a SEM image of the spherical lithium manganese iron phosphate positive electrode material prepared in Example 1 of the present application;

[0035] Figure 3 This is a SEM image of the lithium manganese iron phosphate positive electrode material prepared in Comparative Example 4 of the present application;

[0036] Figure 4This is a first cycle charge and discharge curve diagram of a modified spherical lithium manganese iron phosphate positive electrode material obtained in Example 1 of the present application. DETAILED DESCRIPTION

[0037] To facilitate the understanding of the present application, the present application will be described in more comprehensive and detailed manner below in conjunction with the accompanying drawings and preferred embodiments of the specification, but the protection scope of the present application is not limited to the following specific embodiments.

[0038] Unless otherwise defined, all professional terms used below have the same meaning as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of this application.

[0039] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0040] A method for preparing a spherical lithium manganese iron phosphate positive electrode material comprises the following steps: Figure 1 As shown:

[0041] S1, mixing a manganese source, an iron source, a doping ion M source and a solvent to obtain a first solution;

[0042] S2, mixing a phosphorus source, a lithium source and a solvent to obtain a second solution;

[0043] S3, mixing the first solution obtained in step S1 with the second solution obtained in step S2 to obtain a third solution;

[0044] S4, subjecting the third solution to a hydrothermal reaction, and filtering, washing, and drying to obtain a first spherical lithium manganese iron phosphate positive electrode material;

[0045] S5, mixing the first spherical lithium manganese iron phosphate positive electrode material with a carbon source and a fast ion conductor lithium titanium aluminum phosphate to obtain a calcined precursor;

[0046] S6. calcining the calcined precursor to obtain a second spherical lithium manganese iron phosphate positive electrode material compositely coated with carbon and a fast ion conductor.

[0047] The present application uses the structural guiding effect of ethylene glycol to control the morphology under high temperature and high pressure to form a micron-shaped spherical lithium iron manganese phosphate positive electrode material formed by self-assembly of nanoparticles. Ethylene glycol is used as a structural guiding agent. The molecular structure of ethylene glycol contains two symmetrical hydroxyl groups, which can interact with the surface of the material to form an organic molecular protective layer. This protective layer not only affects the adsorption and growth behavior of surface atoms, but also can regulate the growth rate and orientation of the material to a certain extent. By controlling the amount and time of addition of ethylene glycol, precise control of the material morphology can be achieved. In addition, ethylene glycol will be preferentially adsorbed on areas with higher chemical energy on the surface of the material (such as sharp edges), thereby reducing the surface free energy of these areas. This adsorption will inhibit the continued growth of these areas. Multiple effects lead to a change in the material morphology, allowing the lithium iron manganese phosphate positive electrode material to form a spherical morphology only through a hydrothermal reaction. The self-assembled structure of the nanoparticles increases the tap density of the spherical lithium iron manganese phosphate positive electrode material, making it easier to process, thereby increasing the volume energy density of the lithium battery. At the same time, since the sphere is self-assembled from nanoparticles and has voids inside, the carbon source and the fast ion conductor lithium aluminum titanium phosphate are mixed to form a precursor by calcining the first spherical lithium iron manganese phosphate positive electrode material with a carbon source and a fast ion conductor, The carbon source and the fast ion conductor material enter the interior of the spherical structure. A three-dimensional network structure of electrons and ions is formed in the gaps, which improves the electronic conductivity and ion conductivity of the lithium iron manganese phosphate positive electrode material; and carbon and fast ion conductor materials are also coated on the surface of the lithium iron manganese phosphate positive electrode material, further improving the structural stability of the material; in addition, ion doping improves the intrinsic electronic conductivity, ion conductivity and crystal structure stability of the spherical lithium iron manganese phosphate positive electrode material, and the kinetics of ion deintercalation reaction are fast; thereby, the crystal structure and surface structure are stable while having high electronic conductivity and ion conductivity, and have excellent cycle performance and rate performance, and at the same time, the material has both high volume energy density and good processing performance, and the process is simple and controllable, low energy consumption, low cost, and suitable for large-scale industrial production.

[0048] In one embodiment, the manganese source in S1 includes any one or more combinations of manganese sulfate, manganese nitrate, manganese carbonate, manganese acetate and manganese oxalate; the iron source includes any one or more combinations of iron sulfate, iron nitrate, iron acetate, iron citrate and iron oxalate; the doped ion M source includes any one or more combinations of sulfate, nitrate, acetate, oxalate and citrate, and the sulfate, nitrate, acetate, oxalate and citrate all include Mg, Cu, Ni, Co, Zn, Ca, Y, Al, Ga, Zr, Ti, Cr, Mo, W, Nb or V elements; the manganese source, iron source and doped ion M source are diversified, which reduces the production cost, the doped ion source can provide more conductive ions, stabilize the crystal structure, broaden the lithium ion diffusion channel, and improve the ionic conductivity of the spherical manganese iron phosphate lithium positive electrode material.

[0049] In one embodiment, the phosphorus source in S2 includes any one or more combinations of phosphoric acid, ammonium dihydrogen phosphate and diammonium hydrogen phosphate; the lithium source includes any one or more combinations of lithium hydroxide, lithium nitrate, lithium carbonate, lithium dihydrogen phosphate and lithium phosphate; the sources of phosphorus source and lithium source are diversified, which reduces production costs.

[0050] In one embodiment, the temperature of the hydrothermal reaction in S4 is 200°C~250°C, the reaction time is 9 h~24 h, and the volume ratio of water to ethylene glycol in the hydrothermal reaction system is 1:(0.1-10); the molar ratio of elements Li:Mn:Fe:P:M in the first spherical lithium manganese iron phosphate positive electrode material is (0.9~1.1):(0.1~0.9):(0.1~0.9):1:(0~0.1), and the D50 particle size of the first spherical lithium manganese iron phosphate positive electrode material is 1 μm~5 μm; the morphology is controlled by setting the temperature and time of the hydrothermal reaction to form a micron-sized first spherical lithium manganese iron phosphate positive electrode material self-assembled from nanoparticles, and the molar ratio of each element in the first spherical lithium manganese iron phosphate positive electrode material is controlled to avoid excessive proportion of some elements.

[0051] In one embodiment, the carbon source in S5 is any one or more of sucrose, glucose, fructose, polyethylene glycol, starch, citric acid, ascorbic acid, conductive carbon black, graphene, carbon nanotubes and asphalt; the D50 particle size of the fast ion conductor lithium aluminum titanium phosphate is 0.05 μm to 1 μm. The carbon source coated nanoparticles self-assemble into micron spherical lithium iron manganese phosphate positive electrode material, which improves the electronic conductivity of the spherical lithium iron manganese phosphate positive electrode material; and the fast ion conductor lithium aluminum titanium phosphate (LATP) has the advantages of high ionic conductivity, wide electrochemical window, air stability, and low cost. The surface modification of lithium iron manganese phosphate by LATP makes the spherical lithium iron manganese phosphate positive electrode material have a more stable surface structure, inhibits side reactions on the surface of the material, and isolates the direct contact between the spherical lithium iron manganese phosphate positive electrode material and the electrolyte, slows down the dissolution of manganese ions, and can effectively improve the ionic conductivity of the spherical lithium iron manganese phosphate positive electrode material, reduce material polarization, and thus improve the comprehensive electrochemical performance of the spherical lithium iron manganese phosphate positive electrode material.

[0052] In one embodiment, the content of conductive carbon in the second spherical lithium manganese iron phosphate positive electrode material is 1 wt% to 10 wt%; the content of lithium titanium aluminum phosphate is 0.1 wt% to 5 wt%.

[0053] In one embodiment, the calcination parameters in S6 are: calcination temperature is 600 ℃ ~ 800 ℃, calcination time is 2 h ~ 12 h, and the inert gas in the calcination atmosphere is a combination of one or more of nitrogen, argon, helium, neon, krypton or xenon; by calcining the first spherical lithium iron manganese phosphate positive electrode material and mixing it with a carbon source and a fast ion conductor lithium titanium aluminum phosphate to form a precursor, the carbon source and the fast ion conductor material enter the internal voids of the spherical structure to form a three-dimensional electron-conducting and ion-conducting network structure, thereby improving the conductivity of the spherical lithium iron manganese phosphate positive electrode material, and the composite coating layer formed by carbon and the fast ion conductor lithium titanium aluminum phosphate can further improve the structural stability of the material.

[0054] In a second aspect, the present application further provides a spherical lithium manganese iron phosphate positive electrode material prepared by the preparation method of the spherical lithium manganese iron phosphate positive electrode material as described in any one of the contents of the first aspect.

[0055] In a third aspect, the present application also provides an application of the spherical lithium manganese iron phosphate positive electrode material as described in the second aspect, for preparing a positive electrode sheet.

[0056] In a fourth aspect, the present application further provides a lithium battery, wherein the lithium-ion battery comprises a positive electrode plate as described in the third aspect.

[0057] It can be understood that the beneficial effects of the second to fourth aspects mentioned above can be found in the relevant description of the first aspect mentioned above, and will not be repeated here.

[0058] In order to enable the above implementation details and operations of the present application to be clearly understood by those skilled in the art, and to enable the solution of the present application to be significantly embodied, the above technical solution is illustrated by means of multiple embodiments below.

[0059] Embodiment 1:

[0060] This embodiment provides a method for preparing a spherical lithium manganese iron phosphate positive electrode material, comprising the following steps:

[0061] (1) Manganese sulfate, iron sulfate, and magnesium sulfate are dissolved in ascorbic acid solution at a molar ratio of n(Mn):n(Fe):n(Mg) = 0.6:0.39:0.01. Ascorbic acid acts as a reducing agent to prevent Fe 2+ Oxidized to Fe 3+ , obtaining a first solution; dissolving lithium hydroxide and phosphoric acid in deionized water at a molar ratio of n(Li):n(PO4)=3:1 to obtain a second solution; adding the first solution to the second solution to make n(Li):n(Mn):n(Fe):n(Mg):n(PO4)=3:0.6:0.39:0.01:1, adding ethylene glycol to make a volume ratio of ethylene glycol to deionized water of 4:1, stirring and mixing to obtain a third solution;

[0062] (2) The third solution was subjected to hydrothermal reaction at 210 °C for 12 h, and then filtered, washed, and dried to obtain spherical LiMn 0.6 Fe 0.39 Mg 0.01 PO4 positive electrode material;

[0063] (3) Weigh 10g of spherical LiMn 0.6 Fe 0.39 Mg 0.01 PO4 cathode material, 3 g glucose, and 0.1 g lithium aluminum titanium phosphate (LATP) were mixed evenly to prepare a calcined precursor;

[0064] (4) The precursor was calcined at 800°C for 5 h in a nitrogen atmosphere at a heating rate of 5°C / min. After cooling in the furnace, a modified spherical lithium manganese iron phosphate positive electrode material was obtained. 50 3 μm.

[0065] The SEM image of the spherical lithium manganese iron phosphate positive electrode material obtained in Example 1 is as follows Figure 2 As shown, Figure 2 It shows that the size of the prepared spherical lithium manganese iron phosphate positive electrode material is about 3 μm, which is self-assembled by nanoparticles and there are voids in the spherical structure.

[0066] Embodiment 2:

[0067] This embodiment provides a method for preparing a spherical lithium manganese iron phosphate positive electrode material, comprising the following steps:

[0068] (1) Manganese sulfate, iron sulfate, and magnesium sulfate are dissolved in ascorbic acid solution at a molar ratio of n(Mn):n(Fe):n(Mg) = 0.6:0.39:0.01. Ascorbic acid acts as a reducing agent to prevent Fe 2+ Oxidized to Fe 3+ , obtaining a first solution; dissolving lithium hydroxide and phosphoric acid in deionized water at a molar ratio of n(Li):n(PO4)=3:1 to obtain a second solution; adding the first solution to the second solution to make n(Li):n(Mn):n(Fe):n(Mg):n(PO4)=3:0.6:0.39:0.01:1, adding ethylene glycol to make a volume ratio of ethylene glycol to deionized water of 4:1, stirring and mixing to obtain a third solution;

[0069] (2) The third solution was subjected to hydrothermal reaction at 220°C for 9 hours, and then filtered, washed, and dried to obtain spherical LiMn 0.6 Fe 0.39 Mg 0.01 PO4 positive electrode material;

[0070] (3) Weigh 10g of spherical LiMn 0.6 Fe 0.39 Mg 0.01 PO4 positive electrode material, 3g glucose and 0.2g lithium aluminum titanium phosphate (LATP) were mixed evenly to prepare a calcined precursor;

[0071] (4) The sintered precursor was calcined at 700 °C for 10 h in a nitrogen atmosphere with a heating rate of 5 °C / min. After cooling in the furnace, a modified spherical lithium manganese iron phosphate positive electrode material was obtained with a D50 of 4 μm.

[0072] Embodiment 3:

[0073] This embodiment provides a method for preparing a spherical lithium manganese iron phosphate positive electrode material, comprising the following steps:

[0074] (1) Manganese sulfate, iron sulfate, and nickel sulfate are dissolved in ascorbic acid solution at a molar ratio of n(Mn):n(Fe):n(Ni)=0.59:0.4:0.01. Ascorbic acid acts as a reducing agent to prevent Fe 2+ Oxidized to Fe 3+ , obtaining a first solution; dissolving lithium hydroxide and phosphoric acid in deionized water at a molar ratio of n(Li):n(PO4)=3:1 to obtain a second solution; adding the first solution to the second solution to make n(Li):n(Mn):n(Fe):n(Ni):n(PO4)=3:0.59:0.4:0.01:1, adding ethylene glycol to make a volume ratio of ethylene glycol to deionized water of 4:1, stirring and mixing to obtain a third solution;

[0075] (2) The third solution was subjected to hydrothermal reaction at 210 °C for 12 h, and then filtered, washed, and dried to obtain spherical LiMn 0.59 Fe 0.4 Ni 0.01 PO4 positive electrode material;

[0076] (3) Weigh 10g of spherical LiMn 0.59 Fe 0.4 Ni 0.01 PO4 positive electrode material, 4 g glucose, and 0.1 g lithium aluminum titanium phosphate (LATP) were mixed evenly to prepare a calcined precursor;

[0077] (4) The precursor was calcined at 750°C for 8 h in a nitrogen atmosphere with a heating rate of 5°C / min. After cooling in the furnace, a modified spherical lithium manganese iron phosphate positive electrode material was obtained with a D50 of 3.5 μm.

[0078] Embodiment 4:

[0079] This embodiment provides a method for preparing a spherical lithium manganese iron phosphate positive electrode material, comprising the following steps:

[0080] (1) Manganese sulfate, iron sulfate, and copper sulfate are dissolved in ascorbic acid solution at a molar ratio of n(Mn):n(Fe):n(Cu)=0.6:0.39:0.01. Ascorbic acid acts as a reducing agent to prevent Fe 2+ Oxidized to Fe 3+ , obtaining a first solution; dissolving lithium hydroxide and phosphoric acid in deionized water at a molar ratio of n(Li):n(PO4)=3:1 to obtain a second solution; adding the first solution to the second solution to make n(Li):n(Mn):n(Fe):n(Cu):n(PO4)=3:0.6:0.39:0.01:1, adding ethylene glycol to make a volume ratio of ethylene glycol to deionized water of 4:1, stirring and mixing to obtain a third solution;

[0081] (2) The third solution was subjected to hydrothermal reaction at 210 °C for 18 h, then filtered, washed, and dried to obtain spherical LiMn 0.6 Fe 0.39 Cu 0.01 PO4 positive electrode material;

[0082] (3) Weigh 10g of spherical LiMn 0.6 Fe 0.39 Cu 0.01 PO4 cathode material, 3 g glucose, and 0.1 g lithium aluminum titanium phosphate (LATP) were mixed evenly to prepare a calcined precursor;

[0083] (4) The precursor was calcined at 800°C for 5 h in a nitrogen atmosphere at a heating rate of 5°C / min. After cooling in the furnace, a modified spherical lithium manganese iron phosphate positive electrode material was obtained. 50 is 4.5 μm.

[0084] Comparative Example 1:

[0085] The difference from Example 1 of the present invention is that lithium aluminum titanium phosphate is not added.

[0086] A method for preparing a lithium manganese iron phosphate positive electrode material comprises the following steps:

[0087] (1) Manganese sulfate, iron sulfate, and magnesium sulfate are dissolved in ascorbic acid solution at a molar ratio of n(Mn):n(Fe):n(Mg) = 0.6:0.39:0.01. Ascorbic acid acts as a reducing agent to prevent Fe 2+ Oxidized to Fe 3+, obtaining a first solution; dissolving lithium hydroxide and phosphoric acid in deionized water at a molar ratio of n(Li):n(PO4)=3:1 to obtain a second solution; adding the first solution to the second solution to make n(Li):n(Mn):n(Fe):n(Mg):n(PO4)=3:0.6:0.39:0.01:1, adding ethylene glycol to make a volume ratio of ethylene glycol to deionized water of 4:1, stirring and mixing to obtain a third solution;

[0088] (2) The third solution was subjected to hydrothermal reaction at 210 °C for 12 h, and then filtered, washed, and dried to obtain spherical LiMn 0.6 Fe 0.39 Mg 0.01 PO4 positive electrode material;

[0089] (3) Weigh 10g of spherical LiMn 0.6 Fe 0.39 Mg 0.01 The PO4 cathode material and 3 g of glucose were mixed evenly to prepare a calcined precursor;

[0090] (4) The precursor was calcined at 800°C for 5 h in a nitrogen atmosphere with a heating rate of 5°C / min. After cooling in the furnace, a spherical carbon-coated lithium manganese iron phosphate positive electrode material was obtained with a D50 of 3 μm.

[0091] Comparative Example 2:

[0092] The difference from Example 1 of the present invention is that no carbon source is added.

[0093] A method for preparing a lithium manganese iron phosphate positive electrode material comprises the following steps:

[0094] (1) Manganese sulfate, iron sulfate, and magnesium sulfate are dissolved in ascorbic acid solution at a molar ratio of n(Mn):n(Fe):n(Mg) = 0.6:0.39:0.01. Ascorbic acid acts as a reducing agent to prevent Fe 2+ Oxidized to Fe 3+ , obtaining a first solution; dissolving lithium hydroxide and phosphoric acid in deionized water at a molar ratio of n(Li):n(PO4)=3:1 to obtain a second solution; adding the first solution to the second solution to make n(Li):n(Mn):n(Fe):n(Mg):n(PO4)=3:0.6:0.39:0.01:1, adding ethylene glycol to make a volume ratio of ethylene glycol to deionized water of 4:1, stirring and mixing to obtain a third solution;

[0095] (2) The third solution was subjected to hydrothermal reaction at 210 °C for 12 h, and then filtered, washed, and dried to obtain spherical LiMn 0.6 Fe 0.39 Mg 0.01 PO4 positive electrode material;

[0096] (3) Weigh 10g of spherical LiMn 0.6 Fe 0.39 Mg 0.01 The PO4 cathode material and 0.1 g of lithium aluminum titanium phosphate (LATP) were uniformly mixed to prepare a calcined precursor;

[0097] (4) The precursor was calcined at 800°C for 5 h in a nitrogen atmosphere with a heating rate of 5°C / min. After cooling in the furnace, a spherical lithium titanium aluminum phosphate-coated lithium manganese iron phosphate positive electrode material was obtained with a D50 of 3 μm.

[0098] Comparative Example 3:

[0099] The difference from Example 1 of the present invention is that no carbon source and lithium aluminum titanium phosphate are added for coating.

[0100] A method for preparing a lithium manganese iron phosphate positive electrode material comprises the following steps:

[0101] (1) Manganese sulfate, iron sulfate, and magnesium sulfate are dissolved in ascorbic acid solution at a molar ratio of n(Mn):n(Fe):n(Mg) = 0.6:0.39:0.01. Ascorbic acid acts as a reducing agent to prevent Fe 2+ Oxidized to Fe 3+ , obtaining a first solution; dissolving lithium hydroxide and phosphoric acid in deionized water at a molar ratio of n(Li):n(PO4)=3:1 to obtain a second solution; adding the first solution to the second solution to make n(Li):n(Mn):n(Fe):n(Mg):n(PO4)=3:0.6:0.39:0.01:1, adding ethylene glycol to make a volume ratio of ethylene glycol to deionized water of 4:1, stirring and mixing to obtain a third solution;

[0102] (2) The third solution was subjected to hydrothermal reaction at 210 °C for 12 h, and then filtered, washed, and dried to obtain spherical LiMn 0.6 Fe 0.39 Mg 0.01 PO4 precursor;

[0103] (3) Spherical LiMn 0.6 Fe 0.39 Mg 0.01 The PO4 precursor was calcined at 800℃ for 5h in a nitrogen atmosphere with a heating rate of 5℃ / min. After cooling in the furnace, a spherical lithium manganese iron phosphate cathode material was obtained. 50 3 μm.

[0104] Comparative Example 4:

[0105] The difference from Example 1 of the present invention is that no ethylene glycol is added.

[0106] A method for preparing a lithium manganese iron phosphate positive electrode material comprises the following steps:

[0107] (1) Manganese sulfate, iron sulfate, and magnesium sulfate are dissolved in ascorbic acid solution at a molar ratio of n(Mn):n(Fe):n(Mg) = 0.6:0.39:0.01. Ascorbic acid acts as a reducing agent to prevent Fe 2+ Oxidized to Fe 3+ , obtaining a first solution; dissolving lithium hydroxide and phosphoric acid in deionized water at a molar ratio of n(Li):n(PO4)=3:1 to obtain a second solution; adding the first solution to the second solution to make n(Li):n(Mn):n(Fe):n(Cu):n(PO4)=3:0.6:0.39:0.01:1, adding ethylene glycol to make a volume ratio of ethylene glycol to deionized water of 4:1, stirring and mixing to obtain a third solution;

[0108] (2) The third solution was subjected to hydrothermal reaction at 180°C for 6 h, then filtered, washed and dried to obtain LiMn 0.6 Fe 0.39 Mg 0.01 PO4 nanoparticles;

[0109] (3) LiMn 0.6 Fe 0.39 Mg 0.01 PO4 nanomaterials, 3 g glucose, and 0.1 g lithium aluminum titanium phosphate (LATP) were mixed evenly to prepare a calcined precursor;

[0110] (4) The precursor was calcined at 800° C. for 5 h in a nitrogen atmosphere with a heating rate of 5° C. / min, and the modified lithium manganese iron phosphate positive electrode material was obtained after cooling in the furnace.

[0111] The SEM image of the spherical lithium manganese iron phosphate material obtained in this comparative example 4 is as follows Figure 3 As shown, Figure 3 The spherical shape of the medium-spherical lithium manganese iron phosphate material is not obvious, indicating that when the structure-directing agent ethylene glycol is not added, only agglomerated nanoparticles are obtained through the hydrothermal reaction in Comparative Example 4, and the particle size D50 is 100-200 nm.

[0112] 1. Electrochemical performance test:

[0113] The lithium manganese iron phosphate obtained in Examples 1-4 and Comparative Examples 1-4 was used as the positive electrode active material, mixed evenly with acetylene black and polyvinylidene fluoride (PVDF) at a mass ratio of 8:1:1, dispersed in an N-methylpyrrolidone (NMP) solution, coated on an aluminum foil, and vacuum dried overnight at 120°C to obtain a positive electrode sheet. A lithium sheet negative electrode, a PE separator, an organic solvent such as EC / EMC, and a lithium ion electrolyte composed of LiPF6 were used to assemble a CR2025 button cell in a glove box filled with high-purity argon.

[0114] The battery was subjected to an electrochemical performance test, and the test results are shown in Table 1:

[0115] .

[0116] It can be seen from Table 1 that Examples 1-4 have higher specific capacity and cycle performance than Comparative Examples 1-4. Figure 4 This is a first cycle charge and discharge curve of a spherical lithium manganese iron phosphate positive electrode material obtained in Example 1 of the present application. From the comparison between Example 1 and Comparative Example 1, it can be seen that Figure 4 The button cell of Example 1 has a capacity retention rate of 95.0% after 100 cycles under 1C conditions, while that of Comparative Example 1 is only 88.6%. This is because LATP is added to the spherical lithium manganese iron phosphate positive electrode material of Example 1, which improves the ionic conductivity of the lithium manganese iron phosphate positive electrode material, reduces the polarization of the material and manganese dissolution, thereby improving the cycle performance and rate performance of the battery.

[0117] By comparing Example 1 and Comparative Example 2, it can be seen that the capacity retention rate of the button cell of Example 1 after 100 cycles under 1C condition is 95.0%, while that of Comparative Example 2 is only 86.2%. This is because conductive carbon is added to the spherical lithium iron manganese phosphate positive electrode material of Example 1, and the conductive carbon material is coated on the surface of the lithium iron manganese phosphate positive electrode material, which improves the electronic conductivity of the lithium iron manganese phosphate material on the one hand, and reduces the side reaction between the active material and the electrolyte on the other hand, thereby improving the cycle performance and rate performance of the battery.

[0118] The embodiments described above are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application, and should all be included in the protection scope of the present application.

Claims

1. A method for preparing a spherical lithium manganese iron phosphate positive electrode material, characterized in that: The following steps are involved: S1, mixing a manganese source, an iron source, a doping ion M source and an ascorbic acid solution to obtain a first solution; S2, mixing a phosphorus source, a lithium source and deionized water to obtain a second solution; S3, mixing the first solution obtained in step S1 with the second solution obtained in step S2 and adding ethylene glycol to obtain a third solution; S4, subjecting the third solution to a hydrothermal reaction, and filtering, washing, and drying to obtain a first spherical lithium manganese iron phosphate positive electrode material; the temperature of the hydrothermal reaction in S4 is 200°C to 250°C, the reaction time is 9 h to 24 h, and in the hydrothermal reaction system, the volume ratio of deionized water to ethylene glycol is 1: (0.1-10); S5, mixing the first spherical lithium manganese iron phosphate positive electrode material with a carbon source and a fast ion conductor lithium titanium aluminum phosphate to obtain a calcined precursor; S6, calcining the calcined precursor to obtain a second spherical lithium manganese iron phosphate positive electrode material compositely coated with carbon and a fast ion conductor; The first spherical lithium iron manganese phosphate positive electrode material is a spherical structure lithium iron manganese phosphate positive electrode material which is self-assembled from nanoparticles and has voids inside. The carbon and fast ion conductor material composite coating is that the carbon and fast ion conductor material are coated on the surface of the lithium iron manganese phosphate positive electrode material, and the carbon source and fast ion conductor material also enter the internal voids of the spherical structure of the lithium iron manganese phosphate positive electrode material.

2. The preparation method according to claim 1, characterized in that: The manganese source includes any one or more combinations of manganese sulfate, manganese nitrate, manganese carbonate, manganese acetate and manganese oxalate; The iron source includes any one or more combinations of ferric sulfate, ferric nitrate, ferric acetate, ferric citrate and ferric oxalate; the doping ion M source includes any one or more combinations of sulfate, nitrate, acetate, oxalate and citrate, and the sulfate, nitrate, acetate, oxalate and citrate all include Mg, Cu, Ni, Co, Zn, Ca, Y, Al, Ga, Zr, Ti, Cr, Mo, W, Nb or V elements.

3. The preparation method according to claim 1, characterized in that: The phosphorus source includes any one or more combinations of phosphoric acid, ammonium dihydrogen phosphate and diammonium hydrogen phosphate; The lithium source includes any one or more combinations of lithium hydroxide, lithium nitrate, lithium carbonate, lithium dihydrogen phosphate and lithium phosphate.

4. The preparation method according to claim 1, characterized in that In S4, the molar ratio of the elements Li:Mn:Fe:P:M in the first spherical lithium manganese iron phosphate positive electrode material is (0.9~1.1):(0.1~0.9):(0.1~0.9):1:(0~0.1), and the D50 particle size of the first spherical lithium manganese iron phosphate positive electrode material is 1 μm~5 μm.

5. The preparation method according to claim 1, characterized in that: The carbon source is any one or more of sucrose, glucose, fructose, polyethylene glycol, starch, citric acid, ascorbic acid, conductive carbon black, graphene, carbon nanotubes and asphalt; The D50 particle size of the fast ion conductor lithium aluminum titanium phosphate is 0.05 μm to 1 μm.

6. The preparation method according to claim 1, characterized in that The content of conductive carbon in the second spherical lithium manganese iron phosphate positive electrode material is 1 wt% to 10 wt%; The content of the lithium aluminum titanium phosphate in the second spherical lithium manganese iron phosphate positive electrode material is 0.1 wt% to 5 wt%.

7. The preparation method according to claim 1, characterized in that The calcination parameters in S6 are: calcination temperature is 600°C to 800°C, calcination time is 2 h to 12 h, and the inert gas in the calcination atmosphere is a combination of one or more of nitrogen, argon, helium, neon, krypton or xenon.

8. A spherical lithium manganese iron phosphate positive electrode material prepared by the preparation method according to any one of claims 1 to 7.

9. An application of the spherical lithium manganese iron phosphate positive electrode material as claimed in claim 8, characterized in that: Used to prepare positive electrode sheets.

10. A lithium battery, characterized in that: The lithium battery comprises the positive electrode sheet as described in claim 9.