Lignin-based hard carbon material and preparation method and application thereof

By desulfurizing and high-temperature treating sodium lignosulfonate, combined with pre-oxidation, segmented carbonization and activation steps, a hard carbon material suitable for sodium-ion battery anodes was prepared, solving the problem of poor sodium storage performance caused by high graphitization and realizing the green and safe application of the material.

CN118561278BActive Publication Date: 2024-11-15CHENGDU LITHIUM ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411052551.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-15
Estimated Expiration
2044-08-02

AI Technical Summary

Technical Problem

The current lignin-based hard carbon materials have a high degree of graphitization, resulting in poor sodium storage performance.

Method used

By desulfurizing sodium lignosulfonate, a precursor is prepared and subjected to high-temperature and high-pressure treatment. Combined with pre-oxidation, segmented carbonization, and reactivation, the microstructure of the material is controlled to form a hard carbon material suitable for sodium-ion battery anode materials.

Benefits of technology

The electrochemical performance of hard carbon materials has been improved, enabling their safe and environmentally friendly application in sodium-ion batteries, avoiding the generation of toxic and harmful gases, and enhancing sodium storage performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118561278B_ABST
    Figure CN118561278B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of sodium ion batteries, and discloses a lignin-based hard carbon material and a preparation method and application thereof; the preparation method comprises the following steps: S1 lignin is subjected to desulfonation and activation I treatment to obtain a precursor I; S2 the precursor I is dissolved in a solvent, hexamethylenetetramine is added, and then subjected to a thermal reaction to obtain a precursor II; S3 the precursor II is subjected to pre-oxidation and segmented carbonization to obtain a hard carbon material. The extracted sodium lignin sulfonate is subjected to a precursor stabilization treatment to increase the degree of crosslinking; at the same time, the microstructure of the sodium lignin sulfonate hard carbon material can be regulated, and the electrochemical performance of the sodium lignin sulfonate used as a hard carbon negative electrode material for sodium ion batteries is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a lignin-based hard carbon material and a preparation method and application thereof. Background Art

[0002] With the rapid development of portable electronic devices and electric vehicles, people have witnessed the commercial potential of electrochemical energy storage. As an element in the same group as lithium, sodium has many similar physical and chemical properties to lithium. In addition, sodium is present in a high content in the earth's crust, has abundant resource reserves, and is low in cost. It can be used as a good substitute for lithium. However, the radius of sodium ions is too large and they cannot form stable compounds with graphite, so graphite cannot be used as the negative electrode material for sodium ion batteries. Therefore, to realize the industrialization of sodium ion batteries, it is necessary to find a low-cost and high-performance negative electrode material.

[0003] Hard carbon has become the most promising negative electrode material for sodium-ion batteries due to its advantages such as excellent physical and chemical properties and low cost. Sodium lignin sulfonate is a by-product in the papermaking industry, and most of it is burned as industrial waste. Sodium lignin sulfonate contains a large amount of sulfur, which will generate toxic, harmful and corrosive substances such as sulfur dioxide and sulfuric acid during high-temperature heating. This not only affects the environment, but also wastes resources. Modified sodium lignin sulfonate can be prepared into hard carbon material and used in sodium-ion battery negative electrodes, which broadens the application range of sodium lignin sulfonate, saves resources and protects the environment. Summary of the invention

[0004] Technical problems solved by the present invention:

[0005] It is used to solve the problems of high graphitization degree and poor sodium storage performance of current lignin-based hard carbon materials.

[0006] The technical solution adopted by the present invention is:

[0007] In view of the above technical problems, the present invention aims to provide a lignin-based hard carbon material and a preparation method and application thereof. The specific contents are as follows:

[0008] First, the present application provides a method for preparing a lignin-based hard carbon material, comprising the following steps:

[0009] S1 lignin is treated with desulfonation and activation I to obtain precursor I;

[0010] Desulfonation: Sodium lignin sulfonate is mixed with alkali solution in a solvent, and after steaming, acid solution I is added, and then heat treatment I is performed to obtain; alkali solution: NaOH solution, 1 mol / L; acid solution: H2SO4 solution, 1 mol / L; steaming: 150~200℃, 1~5h; heat treatment I: 80~100℃, 2~4h;

[0011] Activation I: The desulfonated product is subjected to heat treatment II with 1 mol / L hydrobromic acid to obtain precursor I.

[0012] Heat treatment II: 85-100°C, 2-6h; after heat treatment II, add hexadecyltrimethylammonium bromide to remove the unreacted solvent;

[0013] S2 Precursor I is dissolved in a solvent, hexamethylenetetramine is added, and then subjected to a thermal reaction to obtain precursor II; the solvent is an alcohol solvent, including at least one of ethanol, methanol, isopropanol, and isobutanol; the mass ratio of precursor I to hexamethylenetetramine is 1:0.08~0.15. Thermal reaction: 80~120℃, 8~12h; the thermal reaction is carried out in a high-pressure reactor.

[0014] S3 Precursor II is pre-oxidized and carbonized in stages to obtain a hard carbon material.

[0015] During the pre-oxidation process, air is continuously introduced; the air flow rate is 0.5~2L / min;

[0016] The pre-oxidation adopts staged heating, and the heating rate is maintained at 3°C / min; the staged heating includes stage I, stage II, and stage III; stage I: 140~170°C, 1~3h; stage II: 180~210°C, 1~3h; stage III: 280~320°C, 3~7h; the pre-oxidation is carried out in a rotary kiln, and the rotation speed of the rotary kiln is 0.5~2rpm.

[0017] Staged carbonization: The pre-oxidized product is subjected to pre-carbonization, activation II treatment, and carbonization treatment to obtain a hard carbon material.

[0018] Pre-carbonization: Under inert atmosphere, heat up to 280~320℃ at a rate of 3~8℃ / min and keep warm for 0.5~2h; then heat up to 350~750℃ at a rate of 2~5℃ / min and keep warm for 2~5h.

[0019] Activation II: The pre-carbonized product is placed in a treatment solution (0.5 mol / L potassium hydroxide solution or 1 mol / L zinc chloride solution), subjected to heat treatment III (maintained at 180°C for 6 hours), and then heated to 700~900°C at a rate of 2~5°C / min. After being kept warm for 0.5~2h, CO2 is introduced for activation for 2~3h. The pre-carbonized product is immersed in a potassium hydroxide or zinc chloride solution and dried. In the subsequent carbonization process, potassium hydroxide / zinc chloride can etch the carbon material to form a microporous structure, which has a certain improvement in the sodium storage performance.

[0020] Carbonization: In an inert atmosphere, heat to 1000~1500℃ at a rate of 1~3℃ / min and keep at this temperature for 2~4h, then cool to room temperature.

[0021] Second, the present invention provides a hard carbon material obtained by the above-mentioned preparation method.

[0022] Third, the present invention provides an application of the aforementioned hard carbon material in sodium ion batteries.

[0023] The technical mechanism and beneficial effects adopted by the present invention are as follows:

[0024] (1) By desulfurizing sodium lignin sulfonate, the sulfonic acid groups are reduced, avoiding the generation of toxic and harmful gases such as sulfur dioxide during the subsequent carbonization process, making sodium lignin sulfonate green and providing a safe environment for subsequent processing.

[0025] (2) The extracted sodium lignin sulfonate was subjected to precursor stabilization treatment by adding ethanol and hexamethylenetetramine under high temperature and high pressure. Hexamethylenetetramine will decompose at 100°C to form dimethylolamine and release formaldehyde and ammonia, which can react with the phenolic group of sodium lignin sulfonate and increase the degree of crosslinking.

[0026] (3) Through pre-oxidation, segmented carbonization and re-activation treatment, the microstructure of sodium lignin sulfonate hard carbon material was regulated, and the electrochemical properties of sodium lignin sulfonate as hard carbon material were improved, so that it can be used as a hard carbon material in the field of sodium ion batteries in a green and safe way. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The XRD pattern of the finished product prepared in Example 1;

[0028] Figure 2 This is the SEM image of the sheet prepared in Example 1 (magnification: 1000 times). DETAILED DESCRIPTION

[0029] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0030] 1. Example

[0031] Example 1

[0032] (1) Weigh a certain mass of sodium lignin sulfonate and add it to deionized water, and mix it evenly. Then prepare a 1 mol / L NaOH solution and add it to the sodium lignin sulfonate solution. The mixed solution is reacted at 180°C for 3 hours. The mixed solution after the reaction is mixed evenly with the 1 mol / L sulfuric acid solution prepared in advance, and kept warm at 90°C for 3 hours to obtain the extracted sodium lignin sulfonate. The addition amounts of sulfuric acid solution and NaOH solution are 20% and 7% respectively (based on the weight of sodium lignin sulfonate).

[0033] (2) The extracted sodium lignin sulfonate is placed in a 1 mol / L hydrobromic acid solution for precursor activation treatment, where the amount of hydrobromic acid added is 15% of the total weight of the sodium lignin sulfonate; then, the temperature is first raised to 85°C and kept warm for 2 hours; then hexadecyltrimethylammonium bromide is added, where the amount of addition is 1% of the total weight of the sodium lignin sulfonate; the temperature is continued to be raised to 95°C and kept warm for 4 hours. After cooling to room temperature, the obtained material is filtered, washed and dried to obtain sodium lignin sulfonate after precursor activation.

[0034] (3) The activated sodium lignin sulfonate and ethanol are mixed evenly (the activated sodium lignin sulfonate can be completely dissolved in the ethanol solution), 10% (based on the weight of the activated sodium lignin sulfonate) of hexamethylenetetramine (HMTA) is added thereto, and the mixture is added into a high-pressure reactor, and the mixture is reacted at 120° C. for 12 hours to prepare a precursor.

[0035] (4) Pre-oxidation and segmented carbonization; the precursor is placed in a rotary kiln for pre-oxidation treatment, the speed of the rotary kiln is 0.5~2rpm, and air is continuously introduced during the treatment, and the air flow rate is 1.5L / min. Then, the heating rate is maintained at 3℃ / min, and the temperature is maintained at 150℃, 200℃, and 300℃ for 2 hours, 2 hours, and 5 hours respectively to obtain a pre-oxidized precursor. In an inert atmosphere (nitrogen), the temperature is increased to 300℃ at a heating rate of 5℃ / min and kept warm for 1 hour; then the temperature is increased to 600℃ at a heating rate of 3℃ / min and kept warm for 3 hours. After pre-carbonization, the precursor is immersed in a 1mol / L zinc chloride solution for re-activation treatment, and the re-activation treatment is maintained at 180℃ for 6 hours. Finally, under nitrogen protection, the temperature is increased to 800℃ at a heating rate of 3℃ / min. After stabilization for one hour, carbon dioxide activation gas is introduced for 2-3 hours for final activation. After completion, quickly switch to protective gas (nitrogen). After stabilizing for one hour, maintain the heating rate of 3℃ / min and raise the temperature to 1200℃ and keep it at this temperature for 3 hours, and finally cool to room temperature.

[0036] Example 2

[0037] This embodiment differs from Embodiment 1 in that (4) is not included.

[0038] Example 3

[0039] The difference between this embodiment and embodiment 1 is that no activation treatment is performed after pre-carbonization, that is, no re-activation treatment with zinc chloride solution is performed in (4).

[0040] 2. Comparative Examples

[0041] Comparative Example 1

[0042] This comparative example differs from Example 1 in that (3) is not included.

[0043] Comparative Example 2

[0044] The difference between this comparative example and Example 1 is that after the desulfurization and activation treatment, only a pre-oxidation treatment is performed, that is, the staged carbonization in (4) is not included.

[0045] Comparative Example 3

[0046] The difference between this comparative example and Example 1 is that the precursor is only carbonized in stages, that is, the precursor is directly carbonized after desulfonation, and the carbonization does not include activation (CO2). The carbonization does not include the introduction of carbon dioxide activation gas for 2-3 hours for the final activation.

[0047] 3. Test examples

[0048] The materials prepared in Examples 1-3 and Comparative Examples 1-3 were used as negative electrodes in battery assembly, respectively. The battery assembly was completed in a glove box filled with argon gas. Metal sodium sheets were used as positive electrodes to assemble button batteries. Electrochemical tests were performed using an electrochemical workstation, using a constant current charge and discharge mode, and charging and discharging tests were performed at a current density of 0.1C. The discharge cut-off voltage was 0.05V and the charge cut-off voltage was 2.5V. At the same time, the sample prepared in Example 1 was subjected to XRD measurement and the surface morphology of the sample was observed. The results are as follows: Figure 1 and Figure 2 shown.

[0049] The results are shown in Table 1.

[0050] Table 1

[0051]

[0052] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a lignin-based hard carbon material, characterized in that: The steps include: S1 Sodium lignin sulfonate is subjected to desulfonation and activation I treatment to obtain a precursor I; Activation I: The desulfonation product is subjected to heat treatment II with hydrobromic acid to obtain a precursor I; S2 Precursor I is dissolved in a solvent, hexamethylenetetramine is added, and then subjected to a thermal reaction to obtain precursor II; S3 Precursor II is pre-oxidized and carbonized in stages to obtain a hard carbon material; Staged carbonization: The product after pre-oxidation is subjected to pre-carbonization, activation II treatment, and carbonization treatment; Activation II: The pre-carbonized product is placed in a treatment liquid, subjected to heat treatment III, and then heated to 700-900°C at a rate of 2-5°C / min. After being kept warm for 0.5-2h, CO2 is introduced for activation for 2-3h.

2. The method for preparing a lignin-based hard carbon material according to claim 1, characterized in that: S1 includes features (S1-1): (S1-1) Desulfonation: Sodium lignin sulfonate is mixed with alkali solution in a solvent, and after steaming, acid solution I is added, and then heat treatment I is performed to obtain.

3. The method for preparing a lignin-based hard carbon material according to claim 2, characterized in that: (S1-1) includes at least one of features (S1-1-1) to (S1-1-4): (S1-1-1) Alkali solution: NaOH solution, concentration is 1 mol / L; (S1-1-2) Steaming: 150~200℃, 1~5h; (S1-1-3) Acid solution: H2SO4 solution; concentration is 1 mol / L; (S1-1-4) Heat treatment I: 80~100℃, 2~4h; and / or, S1 includes feature (S1-2), and (S1-2) includes at least one of features (S1-2-1) to (S1-2-3): (S1-2-1) Heat treatment II: 85~100℃, 2~6h; (S1-2-2) After heat treatment II, hexadecyltrimethylammonium bromide is added to remove the unreacted solvent; (S1-2-3) The concentration of hydrobromic acid is 1 mol / L.

4. The method for preparing a lignin-based hard carbon material according to claim 1, characterized in that: S3 includes at least one of features (S3-1) to (S3-2): (S3-1) During the pre-oxidation process, air is continuously introduced; (S3-2) Pre-oxidation adopts staged heating.

5. The method for preparing a lignin-based hard carbon material according to claim 4, characterized in that: (S3-1) includes feature (S3-1-1); (S3-1-1) The air flow rate is 0.5~2L / min; and / or, (S3-2) includes at least one of features (S3-2-1) to (S3-2-3): (S3-2-1) The heating rate is maintained at 3°C / min; (S3-2-2) The staged heating includes stage I, stage II, and stage III; stage I: 140~170℃, 1~3h; stage II: 180~210℃, 1~3h; stage III: 280~320℃, 3~7h; (S3-2-3) Pre-oxidation is carried out in a rotary kiln, and the rotation speed of the rotary kiln is 0.5~2rpm.

6. The method for preparing a lignin-based hard carbon material according to claim 1, characterized in that: (S3-3) includes at least one of features (S3-3-1) to (S3-3-3): (S3-3-1) Pre-carbonization: In an inert atmosphere, heat to 280-320°C at a rate of 3-8°C / min and keep warm for 0.5-2h; then heat to 350-750°C at a rate of 2-5°C / min and keep warm for 2-5h; (S3-3-2) Heat treatment III: maintain at 180°C for 6 hours; (S3-3-3) Carbonization: Under an inert atmosphere, heat to 1000~1500℃ at a rate of 1~3℃ / min, keep at this temperature for 2~4h, and then cool to room temperature.

7. The method for preparing a lignin-based hard carbon material according to any one of claims 1 to 6, characterized in that: S2 includes at least one of features (S2-1) to (S2-4): (S2-1) The solvent is an alcohol solvent; (S2-2) The mass ratio of precursor I to hexamethylenetetramine is 1:0.08~0.15; (S2-3) Thermal reaction: 80~120℃, 8~12h; (S2-4) The thermal reaction is carried out in a high-pressure reactor.

8. The hard carbon material obtained by the preparation method according to any one of claims 1 to 7.

9. Use of the hard carbon material as claimed in claim 8 in sodium ion batteries.