A method for preparing a high performance aluminum nitride ceramic substrate

Through the ball milling dispersion method and the formation of a macromolecular chain liquid phase system, the problems of insufficient strength and low thermal conductivity of traditional aluminum nitride ceramic substrates are solved, and the preparation of aluminum nitride ceramic substrates with high strength, low warpage and high thermal conductivity is achieved. .

CN118561605BActive Publication Date: 2024-10-15FUJIAN HUAQING ELECTRONICS MATERIAL TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411052697.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-10-15
Estimated Expiration
2044-08-02

AI Technical Summary

Technical Problem

Traditional aluminum nitride ceramic substrates have limited strength, are easily warped, have high roughness, and have insufficient thermal conductivity, making it difficult to meet high-performance requirements.

Method used

The sintering slurry is mixed and dispersed using the ball milling dispersion method, and the polymer polyacrylic acid and composite binder are added to form a macromolecular chain liquid phase system. Through the adsorption and bonding of aluminum nitride particles, combined with ultrasonic treatment, the sintering density is improved. sex and intensity.

Benefits of technology

An aluminum nitride ceramic substrate with high strength, small warpage, low roughness and excellent thermal conductivity is prepared to meet the needs of high-performance applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to the technical field of ceramic materials, and in particular to a method for preparing a high-performance aluminum nitride ceramic substrate, comprising the following steps: S1: mixing and dispersing: ball milling and dispersing the sintered slurry to obtain a mixed slurry; S2: tape casting, sheet flattening and debinding; S3: sintering: sending the debinding material into a spark plasma sintering furnace and heating it to 1550-1650°C, and keeping it warm for 30-50 minutes; S4: cooling: cooling the sintered body to room temperature. The method for preparing a high-performance aluminum nitride ceramic substrate of the present invention has good mechanical strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ceramic materials, and in particular to a method for preparing a high-performance aluminum nitride ceramic substrate. Background Art

[0002] At present, the commonly used substrate materials mainly include plastic substrates, metal substrates, ceramic substrates and composite substrates. Ultra-thin composite substrates made of advanced ceramic materials have excellent electrical insulation properties, high thermal conductivity, excellent soft solderability and high adhesion strength, and can be etched with various patterns like PCB boards, and have great current carrying capacity. Ceramic substrates are much better than ordinary glass fiber PCB boards due to their heat dissipation performance, current carrying capacity, insulation, thermal expansion coefficient, etc., and are therefore widely used in high-power power electronic modules, aerospace, military electronics and other products. Traditional aluminum nitride ceramic substrates are obtained by mixing aluminum nitride with sintering aids to form a slurry, and then tape casting, debinding, and sintering. The aluminum nitride ceramic substrates obtained by this process have limited strength, are prone to warping, and have high roughness. The thermal conductivity is still a distance away from the theoretical performance. Therefore, it is of great significance to develop a new method to prepare aluminum nitride ceramic substrates with high strength, low warping, low roughness, and high thermal conductivity. Summary of the invention

[0003] In view of this, an object of the present invention is to provide a method for preparing a high-performance aluminum nitride ceramic substrate, wherein the obtained ceramic substrate has good mechanical strength.

[0004] In order to achieve the above object, the present invention provides the following technical solutions:

[0005] A method for preparing a high-performance aluminum nitride ceramic substrate comprises the following steps:

[0006] S1: Mixing and dispersing: ball milling the sintered slurry to obtain a mixed slurry;

[0007] S2: Casting, flattening and debonding:

[0008] S3: Sintering: The debinded material is sent into a spark plasma sintering furnace and heated to 1550-1650°C for 30-50 minutes;

[0009] S4: Cooling: Cooling the sintered body to room temperature.

[0010] Preferably, the sintering slurry in step S1 comprises polymer polyacrylic acid, a composite binder and aluminum nitride.

[0011] Preferably, the weight ratio of the polymer polyacrylic acid, the composite adhesive and the aluminum nitride is 5:1:4.

[0012] Preferably, the preparation method of the polymer polyacrylic acid specifically comprises the following steps:

[0013] Mix 10% by mass ammonium persulfate, monomer acrylic acid and isopropanol, heat to 60-75°C, stir for 20 minutes, continue to heat to 80-90°C and stir for 1-2 hours, keep warm for 1 hour, and finally cool to room temperature to obtain the polymer polyacrylic acid.

[0014] Preferably, the weight ratio of the ammonium persulfate, the monomer acrylic acid and the isopropyl alcohol is 5:1:2.

[0015] Preferably, the composite adhesive comprises acrylonitrile, ionic liquid and organic acid ester.

[0016] Preferably, the weight ratio of acrylonitrile, ionic liquid and organic acid ester is 5:1:1.

[0017] Preferably, the ionic liquid includes at least one of 1-ethyl-3-methylimidazolium methyl phosphate, 1-ethyl-3-methylimidazolium dihydrogen ammonium salt and 1-ethyl-2,3-dimethylimidazolium hexafluorophosphate.

[0018] Preferably, the organic acid ester includes at least one of isopropyl citrate, tributyl citrate and dioctyl azelate.

[0019] Preferably, the ball milling dispersion in step S1 specifically includes the following steps: a circulation frequency of 700-900 rpm, a diaphragm pump frequency of 50-60 Hz, a sand milling time of 1-2 h, and an ultrasonic frequency of 20-50 Hz.

[0020] The addition of the polymer polyacrylic acid and the composite adhesive of the present invention can form a macromolecular chain liquid phase system, which is beneficial to the rearrangement and growth of aluminum nitride grains through adsorption and bonding of aluminum nitride particles, and can increase the flexibility of the liquid phase system. At the same time, during the dispersion process, ultrasound is used to accelerate and improve the wettability of the macromolecular liquid phase system on the aluminum nitride particles and the surface bonding protection. In the process of forming the macromolecular liquid phase system, voids are generated, making the sintering more dense and the strength better. DETAILED DESCRIPTION

[0021] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention. In addition, it is specifically stated that the raw materials and equipment of the present invention can be obtained from commercial sources, and no longer listed one by one. Among them, the raw materials of the present invention can be obtained from commercial sources and are well known to those skilled in the art. Example 1

[0022] A method for preparing a high-performance aluminum nitride ceramic substrate comprises the following steps:

[0023] S1: Mixing and dispersion: The sintered slurry is dispersed by ball milling, with a circulation frequency of 900 rpm, a diaphragm pump frequency of 60 Hz, a sand milling time of 2 h, and an ultrasonic frequency of 50 Hz to obtain a mixed slurry;

[0024] The sintering slurry includes a polymer polyacrylic acid, a composite binder and aluminum nitride, and is obtained by mixing the polymer polyacrylic acid, the composite binder and the aluminum nitride in a weight ratio of 5:1:4;

[0025] The preparation method of the polymer polyacrylic acid specifically comprises the following steps:

[0026] 10% ammonium persulfate, acrylic acid monomer and isopropanol were mixed in a weight ratio of 5:1:2, and the mixture was heated to 75°C, stirred for 20 minutes, heated to 90°C and stirred for 2 hours, and reacted for 1 hour, and finally cooled to room temperature to obtain a polymer polyacrylic acid.

[0027] The composite adhesive comprises acrylonitrile, ionic liquid and organic acid ester, which are mixed in a weight ratio of 5:1:1; wherein the ionic liquid is 1-ethyl-3-methylimidazolium methyl phosphate; and the organic acid ester is isopropyl citrate;

[0028] S2: Casting, flattening and debonding:

[0029] S3: Sintering: The debinded material is sent into a spark plasma sintering furnace and heated to 1650°C for 50 minutes;

[0030] S4: Cooling: Cooling the sintered body to room temperature. Example 2

[0031] A method for preparing a high-performance aluminum nitride ceramic substrate comprises the following steps:

[0032] S1: Mixing and dispersion: The sintered slurry is dispersed by ball milling, with a circulation frequency of 700 rpm, a diaphragm pump frequency of 50 Hz, a sand milling time of 1 h, and an ultrasonic frequency of 20 Hz to obtain a mixed slurry;

[0033] The sintering slurry includes a polymer polyacrylic acid, a composite binder and aluminum nitride, and is obtained by mixing the polymer polyacrylic acid, the composite binder and the aluminum nitride in a weight ratio of 5:1:4;

[0034] The preparation method of the polymer polyacrylic acid specifically comprises the following steps:

[0035] 10% ammonium persulfate, acrylic acid monomer and isopropanol were mixed in a weight ratio of 5:1:2, and the mixture was heated to 60°C, stirred for 20 minutes, heated to 80°C, stirred for 1 hour, and reacted for 1 hour, and finally cooled to room temperature to obtain a polymer polyacrylic acid.

[0036] The composite adhesive comprises acrylonitrile, ionic liquid and organic acid ester, which are mixed in a weight ratio of 5:1:1; wherein the ionic liquid is 1-ethyl-3-methylimidazolium methyl phosphate; and the organic acid ester is isopropyl citrate;

[0037] S2: Casting, flattening and debonding:

[0038] S3: Sintering: The debinded material is sent into a spark plasma sintering furnace and heated to 1550°C for 30 minutes;

[0039] S4: Cooling: Cooling the sintered body to room temperature. Example 3

[0040] A method for preparing a high-performance aluminum nitride ceramic substrate comprises the following steps:

[0041] S1: Mixing and dispersion: The sintered slurry is dispersed by ball milling, with a circulation frequency of 800 rpm, a diaphragm pump frequency of 55 Hz, a sand milling time of 1.5 h, and an ultrasonic frequency of 30 Hz to obtain a mixed slurry;

[0042] The sintering slurry includes a polymer polyacrylic acid, a composite binder and aluminum nitride, and is obtained by mixing the polymer polyacrylic acid, the composite binder and the aluminum nitride in a weight ratio of 5:1:4;

[0043] The preparation method of the polymer polyacrylic acid specifically comprises the following steps:

[0044] 10% ammonium persulfate, acrylic acid monomer and isopropanol were mixed in a weight ratio of 5:1:2, and the mixture was heated to 65°C, stirred for 20 minutes, heated to 85°C, stirred for 1.5 hours, reacted for 1 hour, and cooled to room temperature to obtain a polymer polyacrylic acid.

[0045] The composite adhesive comprises acrylonitrile, ionic liquid and organic acid ester, which are mixed in a weight ratio of 5:1:1; wherein the ionic liquid is 1-ethyl-3-methylimidazolium methyl phosphate; and the organic acid ester is isopropyl citrate;

[0046] S2: Casting, flattening and debonding:

[0047] S3: Sintering: The debinded material is sent into a spark plasma sintering furnace and heated to 1600°C for 40 minutes;

[0048] S4: Cooling: Cooling the sintered body to room temperature.

[0049] Comparative Example 1:

[0050] The preparation method of Comparative Example 1 is basically the same as that of Example 1, except that aluminum nitride and isopropanol are directly mixed and dispersed, specifically:

[0051] A method for preparing a high-performance aluminum nitride ceramic substrate comprises the following steps:

[0052] S1: Mixing and dispersion: aluminum nitride and isopropanol are mixed and dispersed by ball milling, with a circulation frequency of 900 rpm, a diaphragm pump frequency of 60 Hz, a sand milling time of 2 h, and an ultrasonic frequency of 50 Hz to obtain a mixed slurry; wherein isopropanol is used as a mixed liquid auxiliary agent; the mixing ratio of aluminum nitride and isopropanol is 1:1;

[0053] S2: Casting, flattening and debonding:

[0054] S3: Sintering: The debinded material is sent into a spark plasma sintering furnace and heated to 1650°C for 50 minutes;

[0055] S4: Cooling: Cooling the sintered body to room temperature.

[0056] The following tests were conducted on Examples 1-3, the commercially available ceramic substrates produced by Shenzhen Jiarifeng Electronic Materials Co., Ltd., and the ceramic substrates obtained in Comparative Example 1.

[0057] Performance Testing:

[0058] Warpage test: Use a parallel plate warpage instrument to measure the warpage of the ceramic substrate. The standard spacing of the parallel plates = the standard thickness of the substrate + the allowable warpage value (1.8‰). If the ceramic substrate passes between the parallel plates, it is considered to have passed the warpage test.

[0059] Roughness: Use a roughness meter to measure the roughness of the ceramic substrate.

[0060] Strength: The ceramic substrate is laser scribed into small plates of 24*40mm, and then the substrate strength is tested by fracture extrusion using a universal electronic material testing machine.

[0061] Thermal conductivity: Using LFA467 thermal conductivity tester (10mm*2.0mm specification sample), the qualified thermal conductivity range is ≥170W / (m·K).

[0062] The warpage, roughness and strength were tested on 100 ceramic substrates, and the average value of the test results was taken.

[0063] Table 1: Test data of ceramic substrates of Examples 1-3, commercially available substrates and Comparative Example 1

[0064]

[0065] It can be seen from the above table that the substrates prepared in Examples 1-3 have relatively good warpage, roughness, strength and thermal conductivity.

[0066] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing a high-performance aluminum nitride ceramic substrate, characterized in that: The following steps are involved: S1: Mixing and dispersing: ball milling the sintered slurry to obtain a mixed slurry; S2: Casting, flattening and debonding: S3: Sintering: The debinded material is sent into a spark plasma sintering furnace and heated to 1550-1650°C for 30-50 minutes; S4: Cooling: cooling the sintered body to room temperature; The sintering slurry in step S1 includes a polymer polyacrylic acid, a composite binder and aluminum nitride; The weight ratio of the polymer polyacrylic acid, the composite adhesive and the aluminum nitride is 5:1:4; The preparation method of the polymer polyacrylic acid specifically comprises the following steps: Mix 10% ammonium persulfate, monomer acrylic acid and isopropanol, heat to 60-75°C, stir for 20 minutes, continue to heat to 80-90°C, stir for 1-2 hours, keep warm for 1 hour, and finally cool to room temperature to obtain a polymer polyacrylic acid. The composite adhesive comprises acrylonitrile, ionic liquid and organic acid ester; The ionic liquid includes at least one of 1-ethyl-3-methylimidazolium methyl phosphate, 1-ethyl-3-methylimidazolium dihydrogen ammonium salt and 1-ethyl-2,3-dimethylimidazolium hexafluorophosphate; The weight ratio of the acrylonitrile, the ionic liquid and the organic acid ester is 5:1:

1.

2. The method for preparing a high-performance aluminum nitride ceramic substrate according to claim 1, characterized in that: The weight ratio of the ammonium persulfate, the monomer acrylic acid and the isopropyl alcohol is 5:1:

2.

3. The method for preparing a high performance aluminum nitride ceramic substrate according to claim 1, characterized in that: The organic acid ester includes at least one of isopropyl citrate, tributyl citrate and dioctyl azelate.

4. The method for preparing a high performance aluminum nitride ceramic substrate according to claim 1, characterized in that: The ball milling dispersion in step S1 specifically includes the following steps: a circulation frequency of 700-900 rpm, a diaphragm pump frequency of 50-60 Hz, a sand milling time of 1-2 h, and an ultrasonic frequency of 20-50 Hz.