A high-wettability buffered oxide etching solution, preparation method and application thereof
By adding polyhydroxy alkyl quaternary ammonium salt and photoresist protectant to the buffer oxide etching solution, the problems of unsatisfactory wetting properties and photoresist deformation of the existing BOE etching solution are solved, and high wetting properties and Stable etching effect.
Patent Information
- Application Number
- CN202411034548.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-07-31
Smart Images

Figure CN118562505B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to etching liquid technology, in particular to a high-wettability buffered oxide etching liquid, a preparation method and application thereof. Background Art
[0002] Buffered oxide etchant (BOE) achieves the purpose of etching by removing or thinning the oxide layer of the semiconductor silicon wafer film that is not covered by photoresist. It is often used in microstructure production and silicon-based light-emitting devices.
[0003] BOE etching solution usually uses ultrapure water as solvent, and a certain concentration of HF and NH4F are mixed in a certain proportion to obtain a BOE etching solution of the required proportion. However, the surface tension of the BOE etching solution obtained by the above preparation method is very large, and the wettability of the semiconductor silicon wafer etching layer cannot achieve the desired effect, resulting in severe deformation of the photoresist. In the prior art, the etching wettability and uniformity are often improved by introducing a surfactant into the etching solution. However, due to the characteristics of the BOE etching solution itself, it is difficult to evenly disperse the surfactant in the etching solution, and it usually takes a long time of stirring to ensure that the surfactant is evenly dispersed.
[0004] Therefore, how to obtain a buffered oxide etchant (BOE) with high wettability and low surface tension has become an urgent problem to be solved. Summary of the invention
[0005] The purpose of the present invention is to propose a high-wettability buffered oxide etching solution to address the problem of unsatisfactory wettability of the current BOE etching solution. The etching solution has high wettability and low surface tension, can realize pattern and structure formation in micro-machining and chip manufacturing, and solve the problems of uneven etching and pattern deformation after etching of the existing etching solution.
[0006] It should be noted that, in the present invention, unless otherwise specified, the specific meaning of "including" in relation to composition limitations and descriptions includes both open-ended "including", "comprising", etc. and similar meanings, as well as closed-ended "composed of", "composed of", etc. and similar meanings.
[0007] To achieve the above object, the technical solution adopted by the present invention is: a high wettability buffered oxide etching solution, comprising the following components in weight proportions:
[0008] 5-30 parts of hydrofluoric acid;
[0009] 1-10 parts of polyhydroxyalkyl quaternary ammonium salt;
[0010] 0.1-1 part of photoresist protective agent;
[0011] 1-5 parts of solubilizer;
[0012] Ultrapure water 20-60 parts;
[0013] The polyhydroxyalkyl quaternary ammonium salt is a polyhydroxyalkyl quaternary ammonium salt containing fluoride ions.
[0014] Furthermore, the polyhydroxyalkyl quaternary ammonium salt has a structural formula as shown in Formula I, wherein R1 and R2 are methyl groups; R3 is an alkyl group with 12 to 18 carbon atoms, and R is an alkyl group with 3 to 6 carbon atoms; x and y are both integers, x≥3, y≤x;
[0015]
[0016] Formula Ⅰ.
[0017] Further, where 3≤x≤6.
[0018] The polyhydroxyalkyl quaternary ammonium salt can be dissociated in water to form F - and polyhydroxyalkyl quaternary ammonium ions. The F released after hydrolysis - The F content in the solution can be dynamically adjusted - The concentration of F forms a stable Si-F bond with silicon atoms, ensuring a relatively stable etching rate. - The presence of can buffer the pH value of the etching solution, effectively preventing the abnormal shedding of the photoresist during the wet etching process. Polyhydroxyalkyl quaternary ammonium ions can be used as cationic surfactants, have good solubility and surface activity in aqueous solution, and improve the stability of the solution. It can also produce electrostatic adsorption on the negatively charged SiO2 surface, which can effectively prevent H + Close to the metal surface, thus inhibiting the formation of Si-O-Si and Si-OH, slowing down F - It plays the role of a buffer for the etching of SiO2. At the same time, since the solution contains the same counter ions as the cationic surfactant, the double layer thickness of the surfactant ion end group is compressed, the repulsion between quaternary ammonium ions is reduced, making it easier for them to be closely arranged in the etching solution and to form micelles, which further reduces the surface tension of the etching solution.
[0019] Furthermore, the mass fraction of the hydrofluoric acid is 5-30 parts, for example, 5 parts, 7 parts, 8 parts, 10 parts, 13 parts, 15 parts, 18 parts, 20 parts, 22 parts, 25 parts or 30 parts.
[0020] The mass proportion of the polyhydroxyalkyl quaternary ammonium salt is 1-10 parts, for example, 1 part, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts or 10 parts.
[0021] The mass fraction of the photoresist protective agent is 0.1-1 part, for example, 0.1 part, 0.2 part, 0.3 part, 0.4 part, 0.5 part, 0.6 part, 0.7 part, 0.8 part, 0.9 part or 1 part;
[0022] The mass fraction of the solubilizer is 1-5 parts, for example, 1 part, 2 parts, 3 parts, 4 parts or 5 parts.
[0023] The preparation method of the polyhydroxyalkyl quaternary ammonium salt comprises the following steps: synthesizing polyhydroxy fluoroalkane with epifluoropropane and polyol compounds under the action of isopropanol as a catalyst; 12 ~C 18 ) is reacted at 60-90° C. for 6-10 hours to obtain a polyhydroxyalkyl quaternary ammonium salt.
[0024]
[0025] Furthermore, the polyol compound is one or more of glycerol, D-threitol, xylitol and (2R, 3S, 4R, 5S)-hexane-1,2,3,4,5,6-hexanol.
[0026] Furthermore, the tertiary amine compound is one or more of dodecyl dimethyl tertiary amine, tetradecyl dimethyl tertiary amine, hexadecyl dimethyl tertiary amine and octadecyl dimethyl tertiary amine.
[0027] Furthermore, the molar ratio of epifluoropropane to the polyol compound is 1-3:1-3, for example, 1:1, 1:2, 1:3, 2:1 or 3:1.
[0028] Furthermore, the molar ratio of epifluoropropane to the polyol compound is preferably 1:1.
[0029] Furthermore, the amount of the catalyst isopropanol is 1-3% of the total weight of the catalyst system, for example 1%, 2%, 3%, preferably 1%. In the present invention, % refers to mass percentage unless otherwise specified.
[0030] Furthermore, the molar ratio of the polyhydroxy fluoroalkane to the tertiary amine compound is 1:1-5, such as 1:1, 1:2, 1:3, 1:4 and 1:5.
[0031] Furthermore, the molar ratio of the polyhydroxy fluoroalkane to the tertiary amine compound is preferably 1:1.
[0032] Furthermore, the polyhydroxy fluoroalkane and the tertiary amine compound are reacted at 80° C. for 9 hours to obtain a polyhydroxy alkyl quaternary ammonium salt.
[0033] Furthermore, the photoresist protecting agent is an indene compound.
[0034] Furthermore, the photoresist protecting agent is an indene compound containing hydroxyl groups and amino groups.
[0035] Furthermore, the photoresist protecting agent is one or more of N-[2-(hydroxyamino)-3-nitrosoinden-1-ylidene]hydroxylamine, (1E)-N-hydroxy-6-methoxy-1-indanimine and 1-(4-hydroxy-2,3-dihydro-1H-inden-5-yl)ethanone.
[0036] Furthermore, the photoresist protecting agent is preferably N-[2-(hydroxyamino)-3-nitrosoinden-1-ylidene]hydroxylamine.
[0037] There is a conjugated structure between the benzene ring and the cyclopentadiene ring in the indene compound, so that the molecule has strong stability and conjugated effect, and can effectively resist the erosion and influence of strong acid and strong alkali. The main component of the photoresist is phenolic resin, and the cyclic structure in the indene compound can fill the gap in the resin, especially forming a protective layer at the junction of the resin and silicon dioxide, blocking the etching solution, improving the sealing and stability of the resin, and the stability of the benzene ring structure and the cyclic structure enables the indene compound to stably exist in the etching solution, thereby ensuring a long-term protective effect. At the same time, the indene compound of the present invention also contains hydroxyl and amino, and the hydroxyl and amino in the indene compound form hydrogen bonds with the hydroxyl in the phenolic resin in the photoresist, which can generate attraction between the indene compound molecule and the phenolic resin, and help it to be further adsorbed on the photoresist surface. In addition to hydrogen bonds, van der Waals interactions occur between the aromatic ring structures in the indene compounds and the aromatic ring structures in the phenolic resin, which can enhance the adsorption effect of the indene compounds on the surface of the phenolic resin and play a protective role during the etching process, preventing the photoresist from falling off and deforming after etching.
[0038] Furthermore, the solubilizing agent is one or more of isopropanol, glycerol, diethylene glycol, dipropylene glycol and diethylene glycol.
[0039] Furthermore, the solubilizing agent is preferably isopropanol.
[0040] Another object of the present invention is to disclose a method for preparing a high-wettability buffered oxide etching solution, comprising the following steps:
[0041] Step 1: Weigh each component separately;
[0042] Step 2: Add hydrofluoric acid to ultrapure water and stir, add polyhydroxyalkyl quaternary ammonium salt and continue stirring to obtain reagent A;
[0043] Step 3: dissolving the photoresist protecting agent in the solubilizing agent and stirring to obtain reagent B;
[0044] Step 4: Add reagent B to reagent A and continue stirring to obtain a high wettability buffered oxide etching solution.
[0045] Furthermore, in step 2, hydrofluoric acid is added into ultrapure water at a stirring speed of 60-120 r / min and a stirring time of 60-120 min.
[0046] Furthermore, in step 2, the polyhydroxyalkyl quaternary ammonium salt is added and the stirring time is continued for 60-120 minutes.
[0047] Furthermore, in step 3, the stirring rate is 60-120 r / min, and the stirring time is 30-60 min.
[0048] Furthermore, the stirring time in step 4 is 30-60 min.
[0049] Another object of the present invention is to disclose the application of a high-wettability buffered oxide etching solution in the field of etching a silicon oxide layer on a wafer surface.
[0050] Further, etching the silicon oxide layer on the surface of the wafer using a high wettability buffered oxide etching solution comprises the following steps:
[0051] S1: Place the wafer vertically in a container filled with 25°C high wettability buffered oxide etchant and etch for 1-5 minutes;
[0052] S2: After the etching of S1 is completed, the wafer is placed in ultrapure water for 5-10 minutes and then taken out;
[0053] S3: Purge the wafer surface with high-purity nitrogen for 1-3 minutes to complete the etching process of the silicon oxide layer on the wafer surface.
[0054] Furthermore, the high wettability buffered oxide etching solution in S1 is circulated at a speed of 4-5 L / min.
[0055] Furthermore, the ultrapure water in S2 is circulated at a speed of 4-5 L / min.
[0056] The high wettability buffered oxide etching solution of the present invention, the preparation method and application thereof have the following advantages compared with the prior art:
[0057] 1) The polyhydroxyalkyl quaternary ammonium salt in the high wettability buffered oxide etching solution of the present invention can significantly reduce the surface tension of the etching solution, improve the wettability to the substrate, protect the photoresist during the etching process, and prevent the photoresist from abnormal deformation and falling off; at the same time, it can stabilize F in the etching solution. - Concentration, adjust the pH of the etching solution, play a buffering role in the etching process, and ensure a stable etching rate and uniform etching effect of the etching solution.
[0058] 2) The photoresist protective agent indene compound contained in the high wettability buffered oxide etching solution of the present invention is adsorbed on the photoresist surface by hydrogen bonding and van der Waals force in the etching solution, and the photoresist is prevented from falling off and deforming after etching during the etching process; there is a conjugated structure between the benzene ring and the cyclopentadiene ring in the indene compound, so that the molecule has strong stability and conjugated effect, and can effectively resist the erosion and influence of strong acid and strong alkali. The main component of the photoresist is phenolic resin. The cyclic structure in the indene compound can fill the gap in the resin, especially forming a protective layer at the junction of the resin and silicon dioxide, blocking the etching solution, improving the sealing and stability of the resin, and the stability of the benzene ring structure and the cyclic structure enables the indene compound to exist stably in the etching solution, thereby ensuring a long-term protective effect. The hydroxyl and amino groups in the indene compound form hydrogen bonds with the hydroxyl groups in the phenolic resin in the photoresist, which can generate attraction between the indene compound molecules and the phenolic resin, which helps it to further adsorb on the photoresist surface. In addition to hydrogen bonds, van der Waals interactions occur between the aromatic ring structures in the indene compounds and the aromatic ring structures in the phenolic resin, which can enhance the adsorption effect of the indene compounds on the surface of the phenolic resin and play a protective role during the etching process, preventing the photoresist from falling off and deforming after etching.
[0059] 3) The preparation method of the high wettability buffered oxide etching solution of the present invention has strong operability and is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0060] Figure 1 This is a picture of the chip after etching using the etching solution of Example 1, and the optical microscope magnification is 587 times.
[0061] Figure 2 This is a picture of the chip after etching using the etching solution of Comparative Example 1, and the optical microscope magnification is 587 times.
[0062] Figure 3 This is the infrared spectrum of polyhydroxyalkyl quaternary ammonium salt 1. DETAILED DESCRIPTION
[0063] The present invention is further described below with reference to the examples. The description of the technical features described below is based on representative embodiments and specific examples of the present invention, but the present invention is not limited to these embodiments and specific examples. It should be noted that:
[0064] Unless otherwise stated, the units used in this specification are all international standard units, and the numerical values and numerical ranges appearing in the present invention should be understood to include the inevitable systematic errors in industrial production.
[0065] In this specification, the numerical range expressed using "a numerical value A to a numerical value B" means a range including the endpoints numerical values A and B.
[0066] In the present specification, a numerical range expressed using "above" or "below" means a numerical range including the number.
[0067] In this specification, the word "may" means both performing a certain process and not performing a certain process.
[0068] In this specification, the use of "optional" or "optional" indicates that certain substances, components, execution steps, application conditions and other factors are used or not used.
[0069] In this specification, when "normal temperature" or "room temperature" is used, the temperature may be 15-25°C.
[0070] In this manual, the reagents or instruments used without indicating the manufacturer are all conventional products that can be obtained through commercial purchase.
[0071] Examples 1-5
[0072] Examples 1-5 disclose a variety of high wettability buffered oxide etching solutions, the components and weight ratios of which are shown in Table 1, and the preparation steps are as follows:
[0073] Step 1: Weigh each component in its respective amount;
[0074] Step 2: Add the weighed hydrofluoric acid into deionized water, stir at 100 r / min for 60 min, add polyhydroxyalkyl quaternary ammonium salt, and continue stirring for 100 min to obtain reagent A;
[0075] Step 3: dissolving the photoresist protective agent in the weighed solubilizing agent, stirring at a rate of 100 r / min for 30 min, to obtain reagent B;
[0076] Step 4: Add reagent B to reagent A obtained in step 2, and continue stirring for 30 minutes to obtain a high wettability buffered oxide etching solution.
[0077] Table 1 Components and weight ratios of high wettability buffered oxide etching solutions of Examples 1-5
[0078]
[0079] Among them, the structural formula of the polyhydroxyalkyl quaternary ammonium salt 1-4 is shown in Formula I, wherein R1, R2, R3, R, x and y are selected as shown in Table 2.
[0080]
[0081] Formula I
[0082] The preparation method of the polyhydroxyalkyl quaternary ammonium salt is as follows: using epifluoropropane and polyol compounds as raw materials to synthesize polyhydroxy fluoroalkane under the action of 1% catalyst isopropanol; heating the polyhydroxy fluoroalkane and tertiary amine compounds at 80° C. for 9 hours to obtain the polyhydroxy alkyl quaternary ammonium salt.
[0083] The specific reactions are as follows:
[0084]
[0085] Table 2 Selection of letters in the raw materials and structural formulas of polyhydroxyalkyl quaternary ammonium salts 1-4
[0086]
[0087] Comparative Examples 1-5
[0088] Comparative Examples 1-5 disclose a variety of etching solutions, the components and weight ratios of which are shown in Table 3, and the preparation methods thereof are the same as those of Example 1.
[0089] Table 3 Components and weight ratios of etching solutions in comparative examples 1-5
[0090]
[0091] Among them, the structural formula of quaternary ammonium salt 1 and quaternary ammonium salt 2 is the same as that of polyhydroxyalkyl quaternary ammonium salt 1-4, and the difference is the selection of R1, R2, R3, R, x and y, as shown in Table 4.
[0092] The preparation methods of quaternary ammonium salt 1 and quaternary ammonium salt 2 are the same as those of polyhydroxyalkyl quaternary ammonium salts 1-4, except for the selection of raw materials, as shown in Table 4.
[0093] Table 4 Selection of letters in the raw materials and structural formulas of quaternary ammonium salts 1-2
[0094]
[0095] Various properties of the above-mentioned embodiments 1-5 and comparative examples 1-5 are tested below. The analysis and testing methods are as follows. The test results are shown in Table 5.
[0096] The method of etching the silicon oxide layer on the surface of the wafer using an etching solution is as follows:
[0097] Step 1: Place the etching solution in a 40L chemical tank, maintain the temperature at 25°C, place the wafer vertically in the slot, and circulate the etching solution at a speed of 4L / min;
[0098] Step 2: After the etching of step 1 is completed, the wafer is placed in a chemical tank filled with ultrapure water, in which the ultrapure water is circulated at a speed of 4 L / min, and the wafer is taken out after being placed for 5 minutes;
[0099] Step 3: Purge the wafer surface with high-purity nitrogen at a flow rate of 100L / min for 1-3 minutes to complete the etching process of the silicon oxide layer on the wafer surface.
[0100] Performance Test 1 Surface Tension:
[0101] The surface tension data was measured using a surface tension meter. The test results are shown in Table 5;
[0102] Performance test 2 wettability and photoresist deformation:
[0103] Observe the morphology under an optical microscope, and judge the wettability and photoresist deformation by the morphology after etching. If the wettability is good, there will be no SiO2 residue in the pores and the photoresist will not deform or fall off. Otherwise, the photoresist will fall off seriously. Figure 1 and Figure 2 .
[0104] Performance Test 3 Polyhydroxyalkyl quaternary ammonium salt FTIR:
[0105] Use the ATR accessory to scan the background and remove the impurities, then place a small amount of polyhydroxyalkyl quaternary ammonium salt at the test position and start infrared spectrum scanning. The test results are shown in Figure 3 .
[0106] Table 5 Test results
[0107]
[0108] Referring to Table 5, the test results of the embodiments and comparative examples show that:
[0109] The etching solutions provided in Examples 1-5 of the present invention have a surface tension of less than 30 mN / m, good wetting properties, less damage to the photoresist, and no photoresist falls off.
[0110] Compared with Example 1, Comparative Example 1 did not add polyhydroxyalkyl quaternary ammonium salt, resulting in incomplete wetting and a significant increase in surface tension;
[0111] Compared with Example 1, Comparative Example 2 did not add a protective agent, which resulted in the photoresist falling off and deforming;
[0112] Compared with Example 1, Comparative Example 3 uses ninhydrin as a photoresist protective agent. Since ninhydrin only has a benzene ring and a cyclopentadiene ring, the photoresist partially falls off and the surface tension increases.
[0113] In Comparative Examples 4 and 5, the wettability is reduced and the surface tension is increased due to the change of the quaternary ammonium salt.
[0114] Based on the above content, it can be known that the present invention adopts a combination of polyhydroxyalkyl quaternary ammonium salt and indene-based photoresist protective agent, which can significantly reduce the surface tension of the etching solution, improve the wettability to the substrate, and protect the photoresist from abnormal deformation and shedding during the etching process.
[0115] from Figure 2 It can be seen that Figure 2 The SiO2 etching solution in the circled area is not well soaked, and the etching is uneven. Figure 1 The above problems did not occur in the process, proving that the etching is more uniform after the wettability comparison of the etching solution of the present invention.
[0116] from Figure 3 It can be seen that at 3300nm -1 The broad absorption peaks near can be attributed to the hydroxyl absorption peak, and the absorption peaks of the methylene group are located at 2900nm. -1 and 1200~1400nm -1 Nearby, 1100nm -1 It is the absorption peak area of CF.
[0117] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A high wettability buffered oxide etching solution, characterized in that: The composition includes the following components in weight ratio: 5-30 parts of hydrofluoric acid; 1-10 parts of polyhydroxyalkyl quaternary ammonium salt; 0.1-1 part of photoresist protective agent; 1-5 parts of solubilizer; Ultrapure water 20-60 parts; The polyhydroxyalkyl quaternary ammonium salt is a polyhydroxyalkyl quaternary ammonium salt containing fluoride ions; The structural formula of the polyhydroxyalkyl quaternary ammonium salt is as shown in Formula I, wherein R1 and R2 are methyl groups; R3 is an alkyl group with 12 to 18 carbon atoms, and R is an alkyl group with 3 to 6 carbon atoms; x and y are both integers, x≥3, y≤x; ; The photoresist protecting agent is an indene compound containing hydroxyl and amino groups.
2. The high wettability buffered oxide etching solution according to claim 1, characterized in that: The preparation method of the polyhydroxyalkyl quaternary ammonium salt comprises the following steps: synthesizing polyhydroxy fluoroalkane from epoxy fluoropropane and polyol compounds under the action of isopropanol as a catalyst; reacting the polyhydroxy fluoroalkane and tertiary amine compounds at 60-90° C. for 6-10 hours to obtain the polyhydroxy alkyl quaternary ammonium salt.
3. The high wettability buffered oxide etching solution according to claim 2, characterized in that: The polyol compound is one or more of glycerol, D-threitol, xylitol and (2R,3S,4R,5S)-hexane-1,2,3,4,5,6-hexanol; And / or, the tertiary amine compound is one or more of dodecyl dimethyl tertiary amine, tetradecyl dimethyl tertiary amine, hexadecyl dimethyl tertiary amine and octadecyl dimethyl tertiary amine.
4. The high wettability buffered oxide etching solution according to claim 2, characterized in that: The molar ratio of epifluoropropane to the polyol compound is 1-3:1-3; and / or, the amount of the catalyst isopropanol is 1-3% of the total weight of the catalytic system; And / or, the molar ratio of the polyhydroxy fluoroalkane to the tertiary amine compound is 1:1-5.
5. The high wettability buffered oxide etching solution according to claim 1, characterized in that: The photoresist protecting agent is one or more of N-[2-(hydroxyamino)-3-nitrosoinden-1-ylidene]hydroxylamine, (1E)-N-hydroxy-6-methoxy-1-indanimine and 1-(4-hydroxy-2,3-dihydro-1H-inden-5-yl)ethanone.
6. The high wettability buffered oxide etching solution according to claim 1, characterized in that: The solubilizing agent is one or more of isopropanol, glycerol, diethylene glycol, dipropylene glycol and diethylene glycol.
7. A method for preparing the high wettability buffered oxide etching solution according to any one of claims 1 to 6, characterized in that: The steps include: Step 1: Weigh each component separately; Step 2: Add hydrofluoric acid to ultrapure water and stir, add polyhydroxyalkyl quaternary ammonium salt and continue stirring to obtain reagent A; Step 3: dissolving the photoresist protecting agent in the solubilizing agent and stirring to obtain reagent B; Step 4: Add reagent B to reagent A and stir to obtain a high wettability buffered oxide etching solution.
8. Use of the high wettability buffered oxide etching solution according to any one of claims 1 to 6 in the field of etching silicon oxide layer on the surface of a wafer.
Citation Information
Patent Citations
The cleaning of a glass substrate used in a liquid crystal display, an etching constituent and an etching method using the glass substrate
CN101560058A
Fluorine-containing release agent and preparation method thereof
CN110423202A
Etching compositions
CN111225965A
Water-based capillary crystalline waterproof agent capable of being internally doped and externally sprayed and preparation method thereof
CN115340315A