A g-C3N4 / TiC-added aluminum-bismuth sliding bearing self-lubricating material and preparation method thereof

The aluminum bismuth sliding bearing self-lubricating material was prepared by wrapping g-C3N4 with TiC and mixing it with Bi and Al alloys, which solved the problems of low strength and insufficient self-lubricating performance of the aluminum bismuth sliding bearing material, and significantly improved its dry friction and wear performance and Low temperature tensile properties, suitable for aerospace, new energy vehicles and other fields.

CN118563176BActive Publication Date: 2024-10-15HEFEI UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411036650.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-15
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

Existing aluminum-bismuth sliding bearing materials have problems such as low strength and insufficient self-lubricating performance, which limits their application in aerospace, new energy vehicles and other fields.

Method used

By wrapping g-C3N4 with TiC to form g-C3N4/TiC composite powder, and mixing it with Bi and Al alloy, the self-lubricating aluminum bismuth sliding bearing with g-C3N4/TiC was prepared through ultrasonic stirring, ball milling and plasma sintering. material to improve the dry friction and wear properties and low-temperature tensile properties of the alloy.

Benefits of technology

It effectively improves the self-lubricating performance and friction and wear resistance of Al-Bi alloy, solves the agglomeration problem of g-C3N4 in metal alloys, and maintains excellent tensile strength in extreme low temperature environments, making it suitable for engineering applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118563176B_ABST
    Figure CN118563176B_ABST
Patent Text Reader

Abstract

The present invention relates to a self-lubricating material for aluminum-bismuth sliding bearings with g-C3N4 / TiC added and a preparation method thereof, and belongs to the technical field of new materials. The self-lubricating material for aluminum-bismuth sliding bearings with g-C3N4 / TiC added comprises the following components by mass percentage: TiC: 6%~8%; g-C3N4: 2%~4%; Bi: 20%; the rest is Al. The preparation method of the self-lubricating material for aluminum-bismuth sliding bearings with g-C3N4 / TiC added is to prepare g-C3N4 / TiC powder by stirring TiC powder and g-C3N4 powder in a dispersant while ultrasonically; to prepare Al / Bi powder by mixing Bi powder and Al flakes; to prepare Al / Bi powder by mixing g-C3N4 / TiC powder and Al / Bi powder to prepare Al / Bi mixed powder doped with g-C3N4 / TiC; and to obtain the self-lubricating material for aluminum-bismuth sliding bearings with g-C3N4 / TiC added by pressing and sintering the Al / Bi mixed powder doped with g-C3N4 / TiC. The preparation process of the invention is simple, with few process steps and easy to obtain raw materials; the problem that g-C3N4 is easy to agglomerate and difficult to add into metal alloys is solved; both dry friction and wear performance and tensile performance at low temperatures are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method of adding gC 3 N 4 The invention relates to an aluminum-bismuth sliding bearing self-lubricating material of / TiC and a preparation method thereof, belonging to the technical field of new materials. Background Art

[0002] C 3 N 4 (graphite-like carbon nitride) and TiC (titanium carbide) are promising reinforcement materials in carbonaceous materials and hard particles, respectively.

[0003] TiC has excellent physical properties. Adding TiC to some alloys can improve the strength and wear resistance of the material, and has broad prospects for industrial application. However, directly adding TiC to Al-Bi alloys, TiC as a hard particle can enhance the strength of the alloy, and as a grain refiner can homogenize the Al-Bi alloy, but the dry friction and wear performance is extremely poor, and the low-temperature tensile performance improvement is also poor.

[0004] C 3 N 4 Composed of carbon, nitrogen and hydrogen, gC 3 N 4 Similar to graphite, it has a layered structure. 3 N 4 Directly thermally oxidize and etch in air to destroy the hydrogen bonds in the layer and obtain nanoscale gC 3 N 4 The current research is all gC 3 N 4 In the application of non-metal or material surface, gC 3 N 4 There is no related report on adding TiC into self-lubricating materials of aluminum-bismuth sliding bearings.

[0005] The current aluminum-bismuth sliding bearing materials generally have the disadvantages of low strength and self-lubricating performance that needs to be improved. Therefore, they are rarely used in the fields of aerospace and new energy vehicles. 3 N 4 Get gC 3 N 4 / TiC and adding it to Al-Bi alloy is an effective way to solve this problem.

[0006] Based on this, the present invention is proposed. Summary of the invention

[0007] In view of the shortcomings of the prior art, the present invention provides a method for adding gC 3 N4 / TiC aluminum-bismuth sliding bearing self-lubricating material and preparation method thereof, the specific technical scheme is as follows:

[0008] A kind of gC 3 N 4 The aluminum-bismuth sliding bearing self-lubricating material of / TiC comprises the following components by mass percentage:

[0009] TiC: 6%~8%; gC 3 N 4 : 2%~4%; Bi: 20%; the rest is Al.

[0010] A further improvement is the addition of gC 3 N 4 The aluminum-bismuth sliding bearing self-lubricating material of / TiC comprises the following components by mass percentage:

[0011] TiC: 6%; gC 3 N 4 : 4%; Bi: 20%; the rest is Al.

[0012] A further improvement includes the following components by mass percentage:

[0013] TiC: 8%; gC 3 N 4 : 2%; Bi: 20%; the rest is Al.

[0014] A further improvement, an addition of gC 3 N 4 The method for preparing a self-lubricating material of an aluminum-bismuth sliding bearing of TiC comprises the following steps:

[0015] Step 1: TiC powder, gC 3 N 4 The powder was stirred in a dispersant under ultrasonication and then heated to dryness to obtain gC 3 N 4 / TiC powder;

[0016] Step 2, mixing and grinding Bi powder and Al flakes, and then wet ball milling under argon atmosphere protection, and vacuum drying to obtain Al / Bi powder;

[0017] Step 3: gC 3 N 4 / TiC powder and Al / Bi powder are mixed and stirred to obtain gC 3 N 4 / TiC doped Al / Bi mixed powder;

[0018] Step 4: gC 3N 4 / TiC doped Al / Bi mixed powder was pressed into shape to obtain a sample block;

[0019] Step 5: Place the sample in a graphite mold and perform plasma sintering under vacuum to obtain the gC-added 3 N 4 Aluminum-bismuth / TiC self-lubricating material for sliding bearings.

[0020] In a further improvement, the dispersant is anhydrous ethanol.

[0021] As a further improvement, in step 1, the temperature for heating and evaporating is 80°C and the ultrasonic power is 500W.

[0022] As a further improvement, in step 5, before plasma sintering, the temperature is first increased at a heating rate of 45°C / min to 550°C for sintering, the sintering pressure is 55-60 MPa, and the temperature is kept for 15 minutes.

[0023] As a further improvement, the particle size of the TiC powder is less than or equal to 50 nm, the particle size of the Al flake is less than or equal to 1 μm; and the particle size of the Bi powder is less than or equal to 50 nm.

[0024] The present invention uses TiC to wrap gC 3 N 4 The introduction of Al-Bi alloy not only improves the dry friction and wear properties of the alloy, but also improves the tensile properties at low temperatures.

[0025] C 3 N 4 Under high temperature and high pressure, the structure will be destroyed, or directly damaged by sintering. 3 N 4 The obtained gC 3 N 4 / TiC powder, so that it can exist completely in the Al-Bi alloy, thereby exerting its lubricating properties. 3 N 4 / TiC powder enters the interior of Al-Bi alloy, making TiC, gC 3 N 4 and Bi play a synergistic lubrication role, which is beneficial to the improvement of the self-lubricating properties of the alloy.

[0026] Beneficial effects of the present invention:

[0027] 1. The preparation process of the present invention is simple, with few process steps and easy to obtain raw materials.

[0028] 2. Solved gC 3 N 4It is easy to agglomerate and difficult to add into metal alloys.

[0029] 3. Effectively improve the self-lubricating properties of Al-Bi alloys, adding gC 3 N 4 The application of aluminum-bismuth sliding bearing self-lubricating materials of / TiC in the field of dry friction is possible.

[0030] The study found that: 3 N 4 The density is small, the weight is light, and it is very easy to agglomerate. The wrapping of TiC can promote the spontaneous adsorption of TiC through the dual effects of ultrasonic vibration and stirring during the ultrasonic stirring process. 3 N 4 Around the nanosheet, preventing gC 3 N 4 In addition, gC 3 N 4 It is light and easy to float, making it difficult to add into the alloy. TiC encapsulation solves this problem.

[0031] 4. Adding gC 3 N 4 The aluminum-bismuth sliding bearing self-lubricating material of / TiC has high friction and wear resistance and still has excellent tensile strength under extremely low temperature environment, and is suitable for engineering applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 is a high-power micrograph of the alloy material 1 in Example 1;

[0033] Figure 2 is a high-power micrograph of alloy material 2 in Example 2;

[0034] Figure 3 is a high-power micrograph of alloy material 3 in Example 3;

[0035] Figure 4 is a high-power micrograph of alloy material 4 in Example 4;

[0036] Figure 5 This is a physical picture of the alloy material 1 in Example 1;

[0037] Figure 6 This is a physical picture of alloy material 2 in Example 2;

[0038] Figure 7 This is a physical picture of alloy material 3 in Example 3;

[0039] Figure 8 This is a physical picture of alloy material 4 in Example 4;

[0040] Fig. 9 gC 3 N 4 / TiC powder. DETAILED DESCRIPTION

[0041] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0042] Example 1 (alloy material 1 obtained by adding only TiC)

[0043] 1) Weigh 5g TiC powder, disperse it into 150ml anhydrous ethanol, use an ultrasonic rod to stir for 10min, heat and evaporate to dryness at 80℃ while stirring, and obtain refined TiC powder;

[0044] 2) Weigh 10 g Bi powder and 35 g Al flakes, grind them in an agate mortar, and then perform wet ball milling in a ball mill under argon atmosphere. After the ball milling, vacuum dry the mixture to obtain Al / Bi powder.

[0045] 3) Put 50g of refined TiC powder and Al / Bi powder into a sealed container, rotate and mix at multiple angles for 30 minutes to obtain TiC-doped Al / Bi mixed powder;

[0046] 4) Press the TiC-doped Al / Bi mixed powder into a mold with a pressing weight of 10 tons and hold the pressure for 20-30 seconds to obtain a sample block (cylindrical, 20 mm in diameter, 10 mm in height).

[0047] 5) Place the above sample in a graphite mold and perform plasma sintering under vacuum. Raise the temperature to 550°C at a heating rate of 45°C / min and sinter at a sintering pressure of 55 MPa for 15 minutes. After sintering, an aluminum-bismuth sliding bearing self-lubricating material with TiC added is obtained, referred to as alloy material 1.

[0048] In the alloy material 1, the mass fraction of TiC is 10%, the mass fraction of Bi is 20%, and the mass fraction of Al is 70%.

[0049] 6) Alloy material 1 was tested for friction and wear performance. The friction and wear test was conducted on a CFT-Ⅰ multifunctional material surface comprehensive performance tester. The experimental friction pair was a reciprocating friction mode. Alloy material 1 was cut into sample blocks with a diameter of 18mm and a thickness of 2mm. The GCr15 steel ball (diameter of 5mm, hardness HRC 63-66) was used for the wear part. The load was 1-3N, the running time was 10min, the frequency was 15Hz, and the friction and wear test was conducted under dry friction conditions. See the actual picture of alloy material 1 for details. Figure 5 , wear amount such as Figure 1 shown.

[0050] Example 2 (adding TiC and gC simultaneously 3 N 4 Obtained alloy material 2)

[0051] 1) Weigh 4g TiC powder and 1g gC 3 N 4 The two powders were dispersed in 180 ml of anhydrous ethanol, ultrasonicated and stirred for 10 min using an ultrasonic rod, and heated and evaporated at 80 °C while stirring to obtain gC 3 N 4 / TiC powder; gC 3 N 4 / TiC powder is TiC coated gC 3 N 4 Powder, see Fig. 9 , Fig. 9 TiC coating gC 3 N 4 .

[0052] 2) Weigh 10g Bi powder and 35g Al flakes, grind them in an agate mortar, and then perform wet ball milling in a ball mill under argon atmosphere. After the ball milling, vacuum dry the mixture to obtain Al / Bi powder;

[0053] 3) gC 3 N 4 50g of / TiC powder and Al / Bi powder were placed in a sealed container and mixed and stirred at multiple angles for 60min to obtain gC 3 N 4 / TiC doped Al / Bi mixed powder;

[0054] 4) The above gC 3 N 4 The Al / Bi mixed powder doped with / TiC was pressed into shape with a pressing weight of 10 tons and the pressure was maintained for 20-30s to obtain a sample block (cylindrical, with a diameter of 20mm and a height of 15mm).

[0055] 5) Place the sample block in a graphite mold and perform plasma sintering under vacuum. Sinter at a heating rate of 45°C / min to 550°C. Sinter at a sintering pressure of 55Mpa and keep warm for 15 minutes. After sintering, the gC-added 3 N 4 Aluminum-bismuth sliding bearing self-lubricating material of / TiC, referred to as alloy material 2.

[0056] 6) Alloy material 2 is tested for friction and wear performance. The friction and wear test is carried out on a CFT-Ⅰ multifunctional material surface comprehensive performance tester. The experimental friction pair is a reciprocating friction mode. Alloy material 2 is cut into sample blocks with a diameter of 18mm and a thickness of 2mm. GCr15 steel balls (diameter of 5mm, hardness HRC 63-66) are used for the wear parts. The load is 1-3N, the running time is 10min, the frequency is 15Hz, and the friction and wear test is carried out under dry friction conditions. The actual picture of alloy material 2 is shown in Figure 6 , wear amount such as Figure 2 shown.

[0057] The mass fraction of TiC in alloy material 2 is 8%, gC 3 N 4 The mass fraction of gC is 2%, the mass fraction of Bi is 20%, and the mass fraction of Al is 70%. 3 N 4 The mass fraction of gC / TiC is 10%. 3 N 4 / TiC is TiC encapsulated gC 3 N 4 appears in a compound form.

[0058] Example 3 (adding TiC and gC simultaneously 3 N 4 Obtained alloy material 3)

[0059] 1) Weigh 3g TiC powder and 2g gC 3 N 4 The two powders were dispersed in 200 ml of anhydrous ethanol, ultrasonicated and stirred for 10 min using an ultrasonic rod, and heated and evaporated at 80 °C while stirring to obtain gC 3 N 4 / TiC powder;

[0060] 2) Weigh 10g Bi powder and 35g Al flakes, grind them in an agate mortar, and then perform wet ball milling in a ball mill under argon atmosphere. After the ball milling, vacuum dry the mixture to obtain Al / Bi powder;

[0061] 3) gC3 N 4 50g of TiC / TiC powder and Al / Bi powder were put into a sealed container and mixed and stirred at multiple angles for 50min to obtain gC 3 N 4 / TiC doped Al / Bi mixed powder;

[0062] 4) The above gC 3 N 4 The Al / Bi mixed powder doped with / TiC was pressed into shape with a pressing weight of 10 tons and the pressure was maintained for 20-30s to obtain a sample block (cylindrical, with a diameter of 20mm and a height of 15mm).

[0063] 5) Place the sample block in a graphite mold and perform plasma sintering under vacuum. Sinter at a heating rate of 45°C / min to 550°C. Sinter at a sintering pressure of 55Mpa and keep warm for 15 minutes. After sintering, the gC-added 3 N 4 Aluminum-bismuth sliding bearing self-lubricating material of / TiC, referred to as alloy material 3.

[0064] 6) Alloy material 3 was tested for friction and wear performance. The friction and wear test was conducted on a CFT-Ⅰ multifunctional material surface comprehensive performance tester. The experimental friction pair was a reciprocating friction mode. Alloy material 3 was cut into sample blocks with a diameter of 18mm and a thickness of 2mm. GCr15 steel balls (diameter of 5mm, hardness HRC 63-66) were used for the wear parts. The load was 1-3N, the running time was 10min, the frequency was 15Hz, and the friction and wear test was carried out under dry friction conditions. The actual picture of alloy material 3 is shown in Figure 7 , wear amount such as Figure 3 shown.

[0065] The mass fraction of TiC in alloy material 3 is 6%, gC 3 N 4 The mass fraction of gC is 4%, the mass fraction of Bi is 20%, and the mass fraction of Al is 70%. 3 N 4 The mass fraction of gC / TiC is 10%. 3 N 4 / TiC is TiC encapsulated gC 3 N 4 appears in a compound form.

[0066] Example 4 (adding only gC 3 N 4 Obtained alloy material 4)

[0067] 1) Weigh 5g gC 3 N4 Powder, gC 3 N 4 The powder was dispersed in 200 ml of anhydrous ethanol, and ultrasonicated and stirred for 10 min using an ultrasonic rod, and heated and evaporated to dryness at 80 °C while stirring to obtain refined gC 3 N 4 powder;

[0068] 2) Weigh 10g Bi powder and 35g Al flakes, grind them in an agate mortar, and then perform wet ball milling in a ball mill under argon atmosphere. After the ball milling, vacuum dry the mixture to obtain Al / Bi powder;

[0069] 3) Refined gC 3 N 4 50g of powder and Al / Bi powder were placed in a sealed container and mixed and stirred at multiple angles for 60min to obtain gC 3 N 4 Doped Al / Bi mixed powder;

[0070] 4) The above gC 3 N 4 The doped Al / Bi mixed powder was pressed into a shape with a pressing weight of 10 tons and a pressure holding time of 20-30 seconds to obtain a sample block (cylindrical, 20 mm in diameter, 15 mm in height).

[0071] 5) Place the sample block in a graphite mold and perform plasma sintering under vacuum. Sinter at a heating rate of 45°C / min to 550°C. Sinter at a sintering pressure of 55Mpa and keep warm for 15 minutes. After sintering, the gC-added 3 N 4 Aluminum-bismuth sliding bearing self-lubricating material, referred to as alloy material 4.

[0072] 6) Alloy material 4 was tested for friction and wear performance. The friction and wear test was conducted on a CFT-Ⅰ multifunctional material surface comprehensive performance tester. The experimental friction pair was a reciprocating friction mode. Alloy material 4 was cut into sample blocks with a diameter of 18mm and a thickness of 2mm. GCr15 steel balls (diameter of 5mm, hardness HRC 63-66) were used for the wear parts. The load was 1-3N, the running time was 10min, the frequency was 15Hz, and the friction and wear test was carried out under dry friction conditions. The actual picture of alloy material 4 is shown in Figure 8 , wear amount such as Figure 4 shown.

[0073] Alloy material 4gC 3 N 4 The mass fraction of Si is 10%, the mass fraction of Bi is 20%, and the mass fraction of Al is 70%.

[0074] Characterization test

[0075] Table 1

[0076]

[0077] Table 1 shows the friction and wear performance test results of Examples 1-4. It can be seen that Example 1 is an aluminum-bismuth alloy containing only TiC, while Example 2 contains TiC and gC. 3 N 4 The mass ratio of TiC to gC in the aluminum-bismuth alloy is 4:1. 3 N 4 The mass ratio in the aluminum-bismuth alloy is 3:2. Example 4 contains only gC 3 N 4 Aluminum-bismuth alloy. After comparison, TiC and gC 3 N 4 It can synergistically improve the self-lubricating properties of aluminum-bismuth alloys, adding TiC alone or gC alone 3 N 4 Neither will have this effect.

[0078] Alloy material 1, alloy material 2, alloy material 3, and alloy material 4 were processed into tensile performance test standard parts, respectively, and placed in a freezing instrument for low-temperature treatment. The low-temperature treatment temperature was -80°C, the atmosphere was a vacuum environment, and the low-temperature treatment was performed for 2 hours. Then, the tensile treatment was performed. The results are shown in Table 2:

[0079] Table 2

[0080]

[0081] It can be seen from Table 2 that adding TiC and gC 3 N 4 The obtained alloy materials 3 and 4 have excellent resistance to extreme freezing and can still maintain excellent mechanical properties under extreme freezing conditions.

[0082] In the above embodiment, the particle size of the TiC powder is less than or equal to 50 nm, the particle size of the Al flake is less than or equal to 1 μm; and the particle size of the Bi powder is less than or equal to 50 nm.

[0083] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A self-lubricating material for aluminum-bismuth sliding bearings with g-C3N4 / TiC added, characterized in that: The following components are included by mass percentage: TiC: 6%~8%; g-C3N4: 2%~4%; Bi: 20%; the rest is Al; The method for preparing the aluminum-bismuth sliding bearing self-lubricating material with added g-C3N4 / TiC comprises the following steps: Step 1, stirring TiC powder and g-C3N4 powder in a dispersant while ultrasonicating, and then heating and evaporating to obtain g-C3N4 / TiC powder; Step 2: Mix and grind Bi powder and Al flakes, then perform wet ball milling under argon atmosphere protection, and then vacuum dry to obtain Al / Bi powder; Step 3, mixing and stirring the g-C3N4 / TiC powder and the Al / Bi powder to obtain g-C3N4 / TiC doped Al / Bi mixed powder; Step 4, pressing the g-C3N4 / TiC doped Al / Bi mixed powder into a mold to obtain a sample block; Step 5: Place the sample block in a graphite mold and perform plasma sintering under vacuum to obtain an aluminum-bismuth sliding bearing self-lubricating material with added g-C3N4 / TiC.

2. The aluminum-bismuth sliding bearing self-lubricating material with g-C3N4 / TiC added according to claim 1, characterized in that: The following components are included by mass percentage: TiC: 6%; g-C3N4: 4%; Bi: 20%; the rest is Al.

3. The aluminum-bismuth sliding bearing self-lubricating material with g-C3N4 / TiC added according to claim 1, characterized in that: The following components are included by mass percentage: TiC: 8%; g-C3N4: 2%; Bi: 20%; the rest is Al.

4. A method for preparing a self-lubricating material for aluminum-bismuth sliding bearings with g-C3N4 / TiC added as claimed in any one of claims 1 to 3, characterized in that: The following steps are involved: Step 1, stirring TiC powder and g-C3N4 powder in a dispersant while ultrasonicating, and then heating and evaporating to obtain g-C3N4 / TiC powder; Step 2: Mix and grind Bi powder and Al flakes, then perform wet ball milling under argon atmosphere protection, and then vacuum dry to obtain Al / Bi powder; Step 3, mixing and stirring the g-C3N4 / TiC powder and the Al / Bi powder to obtain g-C3N4 / TiC doped Al / Bi mixed powder; Step 4, pressing the g-C3N4 / TiC doped Al / Bi mixed powder into a mold to obtain a sample block; Step 5: Place the sample block in a graphite mold and perform plasma sintering under vacuum to obtain an aluminum-bismuth sliding bearing self-lubricating material with added g-C3N4 / TiC.

5. The method for preparing a self-lubricating material for aluminum-bismuth sliding bearings with g-C3N4 / TiC added according to claim 4, characterized in that: The dispersant is anhydrous ethanol.

6. The method for preparing a self-lubricating material for aluminum-bismuth sliding bearings with addition of g-C3N4 / TiC according to claim 4, characterized in that: In step 1, the temperature of heating and evaporation is 80° C. and the ultrasonic power is 500W.

7. The method for preparing a self-lubricating material for aluminum-bismuth sliding bearings with addition of g-C3N4 / TiC according to claim 4, characterized in that: In step 5, before plasma sintering, the temperature is raised at a heating rate of 45°C / min to 550°C for sintering, the sintering pressure is 55-60Mpa, and the temperature is kept for 15 minutes.

8. The method for preparing a self-lubricating material for aluminum-bismuth sliding bearings with addition of g-C3N4 / TiC according to claim 4, characterized in that: The particle size of the TiC powder is less than or equal to 50 nm, the particle size of the Al flake is less than or equal to 1 μm; and the particle size of the Bi powder is less than or equal to 50 nm.