A positive electrode material and preparation method thereof, positive electrode sheet and sodium ion battery
By forming a MOF material coating layer on the surface of the layered oxide, the problem of poor interface stability of the layered oxide is solved, the cycle stability and service life of the sodium-ion battery are improved, and side reactions are suppressed by absorbing active oxygen.
Patent Information
- Application Number
- CN202410883456.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-03
AI Technical Summary
The interfacial stability of layered oxides in sodium-ion batteries is poor, which leads to the generation of active oxygen and affects the cycle performance of the battery. The existing dry coating method has limited uniformity and cannot completely suppress the generation of active oxygen.
The MOF material coating layer is used to form a uniform metal organic framework coating layer on the surface of the layered oxide, and the organic ligands in the first metal coordination compound such as triethylenediamine and its derivatives are used to absorb reactive oxygen species and inhibit occurrence of side effects.
It improves the cycle stability and service life of the battery, effectively inhibits the release of active oxygen and other side reactions through the uniform coating layer, and enhances the stability of the cathode material.
Smart Images

Figure CN118572089B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of sodium ion batteries, and in particular, to a positive electrode material and a preparation method thereof, a positive electrode sheet and a sodium ion battery. Background Art
[0002] Among the three major positive electrode materials for sodium-ion batteries, layered oxides have the highest energy density, simple synthesis process, good compatibility of production lines with lithium battery ternary materials, and are relatively mature. However, due to their structural characteristics, layered oxides have poor interface stability and are prone to produce reactive oxygen, resulting in a decrease in cycle performance. A common method is to coat the surface of the layered oxide to reduce the material interface and inhibit the occurrence of side reactions. However, the commonly used dry coating method has limited uniformity, and can usually only achieve point or island coating, which cannot completely inhibit the generation of reactive oxygen, and thus has a negative impact on the cycle stability of the battery. Summary of the invention
[0003] The purpose of the present disclosure is to provide a positive electrode material and a preparation method thereof, a positive electrode sheet and a sodium ion battery. The layered oxide surface of the positive electrode material has a uniform MOF material coating layer, which can absorb the generated active oxygen while inhibiting the generation of active oxygen, thereby effectively improving the cycle stability of the battery.
[0004] In order to achieve the above-mentioned object, the present disclosure provides a positive electrode material in a first aspect, comprising a layered oxide as a core and a MOF material coating layer coated on the surface of the layered oxide; the MOF material coating layer comprises a first metal coordination compound, and the organic ligand of the first metal coordination compound comprises a compound having a structure represented by the following formula (1):
[0005] Formula (1); wherein R1 to R6 are the same or different and are independently selected from one of hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkenyl group having 1 to 10 carbon atoms and an alkynyl group having 1 to 10 carbon atoms.
[0006] Optionally, the first metal element in the first metal coordination compound is selected from one or more of Cu, Fe, Mn, Ca, Ni, Co, Cr, Zn, Ti, V, Zr, Mg, Al, Li and Nb;
[0007] The organic ligand in the first metal coordination compound includes a first organic ligand and a second organic ligand, wherein the first organic ligand is selected from one or more of isophthalic acid, phthalic acid, terephthalic acid, trimesic acid, 1,2,4-benzenetricarboxylic acid and 1,3,5-benzenetricarboxylic acid; the second organic ligand includes a compound of the structure shown in the above formula (1), wherein R1 to R6 are the same or different and are independently selected from one of hydrogen, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, vinyl, propenyl, allyl, butylene, butadienyl, ethynyl, propargyl and butylene;
[0008] The layered oxide includes a compound having a composition represented by the following formula (2):
[0009] Na x TmO2 formula (2); wherein Tm is a second metal element, and Tm is selected from one or more of Cu, Fe, Mn, Ca, Ni, Co, Cr, Zn, Ti, V, Zr, Mg, Al, Li and Nb; the structure of the layered oxide is selected from one or more of P2 type, O3 type, P3 type and tunnel type, 0 <x≤1。
[0010] Optionally, based on the total weight of the positive electrode material, the content of the layered oxide is 58-99.9 wt %, and the content of the MOF material coating layer is 0.1-42 wt %; preferably, the content of the layered oxide is 86.0-99.9 wt %, and the content of the MOF material coating layer is 0.1-14.0 wt %;
[0011] Based on the total weight of the MOF material coating layer, the content of the first metal element is 5-50 weight %, the content of the first organic ligand is 15-60 weight %, and the content of the second organic ligand is 15-60 weight %; preferably, the content of the first metal is 10-40 weight %, the content of the first organic ligand is 20-50 weight %, and the content of the second organic ligand is 20-50 weight %.
[0012] Optionally, the particle size of the positive electrode material is 2.1-23 μm; the particle size of the layered oxide is 2-20 μm; and the thickness of the MOF material coating layer is 0.1-4 μm, preferably 0.1-3 μm.
[0013] A second aspect of the present disclosure provides a method for preparing a positive electrode material, comprising the following steps:
[0014] The layered oxide, the first metal source and the organic ligand are contacted and reacted in a solvent; wherein the organic ligand comprises a compound having a structure represented by the following formula (1):
[0015] Formula (1); wherein R1 to R6 are the same or different and are each independently selected from one of hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkenyl group having 1 to 10 carbon atoms, and an alkynyl group having 1 to 10 carbon atoms.
[0016] Optionally, the first metal source is selected from one or more of nitrates, sulfates, halide salts, and phosphates of a first metal element; the first metal element is selected from one or more of Cu, Fe, Mn, Ca, Ni, Co, Cr, Zn, Ti, V, Zr, Mg, Al, Li, and Nb;
[0017] The layered oxide has the composition shown in the following formula (2):
[0018] Na x TmO2 Formula (2); wherein Tm is a second metal element, and Tm is selected from one or more of Cu, Fe, Mn, Ca, Ni, Co, Cr, Zn, Ti, V, Zr, Mg, Al, Li, and Nb; the structure of the layered oxide is selected from one or more of P2 type, O3 type, P3 type, and tunnel type, 0 < x ≤ 1; the particle size of the layered oxide is 2 to 20 μm;
[0019] The organic ligand includes a first organic ligand and a second organic ligand. The first organic ligand is selected from one or more of isophthalic acid, phthalic acid, terephthalic acid, mellitic acid, 1,2,4-benzenetricarboxylic acid, and 1,3,5-benzenetricarboxylic acid; the second organic ligand has the structure shown in the above formula (1), wherein R1 to R6 are the same or different and are each independently selected from one of hydrogen, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, vinyl, propenyl, allyl, butenyl, butadienyl, ethynyl, propargyl, and butynyl;
[0020] The solvent is selected from one or more of acetonitrile, ethanol, ethylene glycol, methanol, propanol, tetrahydrofuran, and N, N-dimethylformamide.
[0021] Optionally, the weight ratio of the layered oxide: the first metal source: the first organic ligand: the second organic ligand is 1000: 0.05 to 70: 0.15 to 84: 0.15 to 84; preferably 1000: 1 to 48: 2 to 60: 2 to 60.
[0022] Optionally, the conditions for the contact reaction include: in a solvent thermal reaction kettle, the reaction temperature is 100 to 300 °C, and the reaction time is 5 to 36 h.
[0023] The third aspect of the present disclosure provides a positive electrode material prepared by the method according to the second aspect of the present disclosure.
[0024] A fourth aspect of the present disclosure is a positive electrode sheet of a sodium ion battery, comprising the positive electrode material described in the first aspect or the third aspect of the present disclosure.
[0025] A fifth aspect of the present disclosure provides a sodium ion battery, which includes the positive electrode sheet described in the fourth aspect of the present disclosure.
[0026] Through the above technical scheme, the present disclosure provides a positive electrode material and a preparation method thereof, a positive electrode sheet and a sodium ion battery. The positive electrode material provided by the present disclosure includes a layered oxide as a core and a MOF material coating layer coated on the surface of the layered oxide. The MOF material coating layer has a dual role: on the one hand, the MOF material coating layer can achieve a uniform coating effect, which can effectively inhibit the release of active oxygen in the lattice of the positive electrode active material (layered oxide) and the occurrence of other side reactions; on the other hand, the first metal coordination compound in the MOF material includes a compound having a structure shown in formula (1) (such as triethylenediamine and its derivatives) as an organic ligand, and the organic ligand can absorb active oxygen generated by other pathways (such as residual alkali decomposition, sodium salt hydrolysis caused by side reactions, etc.), which can further inhibit the occurrence of side reactions. The positive electrode material provided by the present disclosure can effectively improve the battery cycle stability and extend the service life in the application of sodium ion batteries.
[0027] Other features and advantages of the present disclosure will be described in detail in the following detailed description. DETAILED DESCRIPTION
[0028] The specific embodiments of the present disclosure are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present disclosure, and are not used to limit the present disclosure.
[0029] The first aspect of the present disclosure provides a positive electrode material, comprising a layered oxide as a core and a MOF material coating layer coated on the surface of the layered oxide; the MOF material coating layer comprises a first metal coordination compound, and the organic ligand of the first metal coordination compound comprises a compound having a structure represented by the following formula (1):
[0030] Formula (1); wherein R1 to R6 are the same or different and are independently selected from hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkenyl group having 1 to 10 carbon atoms or an alkynyl group having 1 to 10 carbon atoms.
[0031] The present disclosure provides a positive electrode material, including a layered oxide as a core and a MOF material coating layer coated on the surface of the layered oxide, wherein the MOF material coating layer has a dual role: on the one hand, the MOF material coating layer can achieve a uniform coating effect, and can effectively inhibit the release of active oxygen in the lattice of the positive electrode active material (layered oxide) and the occurrence of other side reactions; on the other hand, the first metal coordination compound in the MOF material includes a compound having a structure shown in formula (1) (such as triethylenediamine and its derivatives) as an organic ligand, and the organic ligand can absorb active oxygen generated by other pathways (such as residual alkali decomposition, sodium salt hydrolysis caused by side reactions, etc.), and can further inhibit the occurrence of side reactions. The positive electrode material provided by the present disclosure can effectively improve the battery cycle stability and extend the service life in sodium ion battery applications.
[0032] In a specific embodiment, the first metal element in the first metal coordination compound is selected from one or more of Cu, Fe, Mn, Ca, Ni, Co, Cr, Zn, Ti, V, Zr, Mg, Al, Li and Nb; preferably, it is selected from one or more of Cu, Zn, Zr, Ca, Mn, Ni, Fe, Al, Ti, Nb and Co.
[0033] In one embodiment, the organic ligand includes a first organic ligand and a second organic ligand, wherein the first organic ligand is selected from one or more of isophthalic acid, phthalic acid, terephthalic acid, trimesic acid, 1,2,4-benzenetricarboxylic acid and 1,3,5-benzenetricarboxylic acid; and the second organic ligand includes a compound having a structure shown in the above formula (1). The present disclosure uses a first organic ligand and a second organic ligand in combination, wherein the first organic ligand contributes to the formation of the MOF framework.
[0034] In a preferred embodiment, in formula (1), R1 to R6 are the same or different and are independently selected from one of hydrogen, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, vinyl, propenyl, allyl, butylene, butadienyl, ethynyl, propargyl, and butylene. The second organic ligand represented by formula (1) having the group types of R1 to R6 in this embodiment can form a more effective MOF organic coating layer.
[0035] In a specific embodiment, the layered oxide includes a compound having a composition represented by the following formula (2):
[0036] Na xTmO₂ of formula (2); where Tm is a second metal element, and Tm is selected from one or more of Cu, Fe, Mn, Ca, Ni, Co, Cr, Zn, Ti, V, Zr, Mg, Al, Li, and Nb, preferably one or more of Cu, Fe, Mn, Ca, Ni, Co, Zn, Ti, Zr, Mg, Al, Li, and Nb; the structure of the layered oxide is selected from one or more of P2 type, O3 type, P3 type, and tunnel type, 0 < x ≤ 1; preferably, 0.7 ≤ x ≤ 1. In the present disclosure, in the same layered oxide, one or more than one metal Tm may be present. The cathode material having the composition shown in formula (2) of this embodiment can have more excellent effects in battery applications.
[0037] In one embodiment, based on the total weight of the cathode material, the content of the layered oxide is 58 to 99.9% by weight, and the content of the MOF material coating layer is 0.1 to 42% by weight; preferably, the content of the layered oxide is 86 to 99.9% by weight, and the content of the metal-organic framework coating layer is 0.1 to 14% by weight; more preferably, the content of the layered oxide is 88 to 99% by weight, and the content of the metal-organic framework coating layer is 1 to 12% by weight. When the content of the active material (layered oxide) and the MOF coating layer in the cathode material of the present disclosure is within the content range of this embodiment, especially within the preferred content range, the cathode material can have a better effect of suppressing the generation of side reactions, suppressing gas production, and absorbing active oxygen, and is more helpful for improving the cycle stability and service life of the battery.
[0038] In one embodiment, based on the total weight of the MOF material coating layer, the content of the first metal element is 5 to 50% by weight, the content of the first organic ligand is 15 to 60% by weight, and the content of the second organic ligand is 15 to 60% by weight; preferably, the content of the first metal is 10 to 40% by weight, the content of the first organic ligand is 20 to 50% by weight, and the content of the second organic ligand is 20 to 50% by weight. When the component content of the MOF material coating layer in the cathode material provided by the present disclosure is within the content range of this embodiment, especially within the optimized range, the cathode material has a better effect of suppressing the generation of active oxygen, reducing the occurrence of side reactions of the cathode material, and absorbing active oxygen, and is more helpful for improving the cycle stability of the battery.
[0039] In one embodiment, the particle size of the positive electrode material is 2-23 μm, preferably 4.2-11 μm; wherein the particle size of the layered oxide is 2-20 μm, preferably 4-10 μm; the thickness of the metal organic framework coating layer is 0.1-4 μm, preferably 0.1-3 μm, more preferably 0.2-1 μm. The positive electrode material provided by the present disclosure has a suitable particle size and coating layer thickness, which is conducive to exerting excellent effects in positive electrode applications.
[0040] A second aspect of the present disclosure provides a method for preparing a positive electrode material, comprising the following steps:
[0041] The layered oxide, the first metal source and the organic ligand are contacted and reacted in a solvent to perform in-situ growth of a metal organic framework material to form a metal organic framework coating layer on the surface of the layered oxide; wherein the organic ligand comprises a compound having a structure represented by the following formula (1):
[0042] Formula (1); wherein R1 to R6 are the same or different and are independently selected from hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkenyl group having 1 to 10 carbon atoms or an alkynyl group having 1 to 10 carbon atoms.
[0043] The present disclosure provides a method for preparing a positive electrode material. The method adopts a wet coating process to in-situ grow a uniform metal organic framework (MOF) coating layer on the surface of an active material layered oxide. The MOF coating layer can effectively inhibit the release of active oxygen in the lattice and the occurrence of other side reactions. The MOF coating layer is prepared by using triethylenediamine (DABCO) and its derivatives shown in formula (1) as ligands. DABCO and its derivatives can also be used to absorb the active oxygen generated by the reaction, thereby achieving the dual effect of the MOF coating layer. The method can also facilitate the control of the product structure of the positive electrode material (such as the thickness of the coating layer) through the conditions of the preparation process. After the MOF coating layer is in-situ grown in the preparation method of the present disclosure, no further heat treatment is required to ensure that the organic ligand can be retained on the surface of the multilayer oxide.
[0044] In a specific embodiment, the first metal source is selected from one or more of nitrates, sulfates, halides and phosphates of a first metal element; the first metal element is selected from one or more of Cu, Fe, Mn, Ca, Ni, Co, Cr, Zn, Ti, V, Zr, Mg, Al, Li and Nb, preferably, the first metal element is selected from one or more of Cu, Zn, Zr, Ca, Mn, Ni, Fe, Al, Ti, Nb and Co; further preferably, the first metal source is selected from one or more of nitrates, halides, sulfides, phosphates or other organic acid salts of the above-mentioned transition metals.
[0045] In a specific embodiment, the layered oxide has the composition shown in the following formula (2):
[0046] Na x TmO2 Formula (2); where Tm is a second metal element, and Tm is selected from one or more of Cu, Fe, Mn, Ca, Ni, Co, Cr, Zn, Ti, V, Zr, Mg, Al, Li, and Nb, preferably one or more of Cu, Fe, Mn, Ca, Ni, Co, Zn, Ti, Zr, Mg, Al, Li, and Nb; the structure of the layered oxide is selected from one or more of P2 type, O3 type, P3 type, and tunnel type, 0 < x ≤ 1; preferably, 0.6 ≤ x ≤ 1. The particle size of the layered oxide is 2 - 20 μm, preferably 5 - 10 μm. The layered oxide provided in this embodiment can obtain a cathode material with better effects.
[0047] In one embodiment, the organic ligand includes a first organic ligand and a second organic ligand. The first organic ligand is selected from one or more of isophthalic acid, phthalic acid, terephthalic acid, mellitic acid, 1,2,4-benzenetricarboxylic acid, and 1,3,5-benzenetricarboxylic acid; the second organic ligand has the structure shown in the above formula (1); where R1 to R6 are the same or different and are each independently selected from one of hydrogen, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, vinyl, propenyl, allyl, butenyl, butadienyl, ethynyl, propargyl, and butynyl.
[0048] In a specific embodiment, the solvent is a solvent that does not react with the layered oxide Na x TmO2, that is, the XRD patterns before and after Na x TmO2 is dispersed in this solvent do not change; preferably, the solvent is selected from one or more of acetonitrile, ethanol, ethylene glycol, methanol, propanol, tetrahydrofuran, and N,N-dimethylformamide.
[0049] In one embodiment, the weight ratio of the layered oxide : the first metal source : the first organic ligand : the second organic ligand is 1000 : 0.05 - 70 : 0.15 - 84 : 0.15 - 84, preferably 1000 : 1 - 48 : 2 - 60 : 2 - 60. According to the optimized raw material ratio provided in this embodiment, especially the preferred raw material ratio, the prepared cathode material can have more excellent performance, which is beneficial to improving the cycle stability of sodium-ion batteries. Optionally, relative to 1 g of the layered oxide, the amount of the solvent used is 2 - 200 mL, preferably 10 - 100 mL. The amount of the solvent used can be adjusted according to the experimental situation.
[0050] In a specific embodiment, the method includes:
[0051] Mixing the layered oxide and a solvent to obtain a suspension;
[0052] Adding a first metal source and an organic ligand into the suspension and mixing them to obtain a reaction mixture;
[0053] The reaction mixture is subjected to a solvothermal reaction to in-situ grow a metal organic framework material on the surface of the layered oxide and form a metal organic framework coating layer;
[0054] The solvothermal reaction product was centrifuged and dried.
[0055] In one embodiment, the contact reaction conditions include: in a solvent thermal reactor, the reaction temperature is 100-300° C., the reaction time is 5-36 hours; the reaction pressure is autogenous pressure;
[0056] Preferably, in the solvent thermal reactor, the reaction temperature is 100-200°C, the reaction time is 8-18h, and the reaction pressure is autogenous pressure. The preferred solvent thermal reaction conditions provided in this embodiment can achieve a better effect of in-situ generation of MOF coating layer.
[0057] A third aspect of the present disclosure provides a positive electrode material prepared according to the method described in the second aspect of the present disclosure.
[0058] A fourth aspect of the present disclosure provides a positive electrode sheet for a sodium ion battery, comprising the positive electrode material described in the first aspect or the third aspect of the present disclosure.
[0059] In a specific embodiment, the positive electrode plate is prepared by a method comprising the following steps: coating a positive electrode slurry on a current collector and then baking and drying; wherein the positive electrode slurry comprises the positive electrode material, an optional binder, an optional conductive agent and a solvent.
[0060] In a preferred embodiment, based on the total weight of the positive electrode slurry, the content of the positive electrode material is 50-100 weight percent, the content of the binder is 0-50 weight percent, and the content of the conductive agent is 0-50 weight percent; the amount of the solvent can be adjusted according to experimental requirements. The positive electrode sheet prepared according to the component content ratio of the positive electrode slurry provided in this embodiment can have better performance.
[0061] In the present disclosure, the binder, the conductive agent and the solvent may be conventional agents in the art.
[0062] In a specific embodiment, the binder is selected from one or more of fluorine-based resins such as polyvinylidene fluoride, polyaniline, polypyrrole, styrene-butadiene copolymer, and acrylic copolymer; the conductive agent is selected from one or more of carbon black, acetylene black, graphene, carbon nanotubes, conductive graphite, and graphite-based conductive agents; and the solvent is selected from one or more of N-methylpyrrolidone and acetone.
[0063] A fifth aspect of the present disclosure provides a sodium ion battery, which includes the positive electrode sheet described in the fourth aspect of the present disclosure.
[0064] The assembly method of the sodium ion battery provided in the present disclosure is a conventional method in the art. The negative electrode material of the sodium ion battery can be hard carbon negative electrode, soft carbon negative electrode, silicon-based negative electrode, sodium metal negative electrode, transition metal sulfide negative electrode or phosphide negative electrode; the electrolyte can be ester electrolyte or ether electrolyte.
[0065] The present disclosure is further described in detail below through examples. The raw materials used in the examples can all be obtained through commercial channels.
[0066] The component contents of the positive electrode material and the component contents of the coating layer in the present disclosure are calculated by the designed stoichiometry;
[0067] The particle size of the positive electrode material and the thickness of the coating layer were measured from the microscopic morphology images obtained by scanning electron microscopy.
[0068] Example 1
[0069] 1g of NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2 (O3 type structure, the second metal element includes Ni, Fe and Mn) is dispersed in 60ml N,N-dimethylformamide, stirred and ultrasonicated to obtain a suspension. 22mg Cu(NO3)2 (first metal source), 30mg terephthalic acid (PTA, first organic ligand), 30mg triethylenediamine (DABCO, second organic ligand) are added to the above suspension, stirred for 30min and ultrasonicated for 30min, wherein the weight ratio of layered oxide: first metal source: first organic ligand: second organic ligand is 1000:22:30:30, and the amount of solvent is 60mL relative to 1g of layered oxide. The suspension is then transferred to a tetrafluoroethylene solvent thermal reactor, and the solvent thermal reactor is placed in a muffle furnace for solvent thermal reaction, the reaction temperature is 150℃, and the reaction time is 12h. After the reaction, the suspension is centrifuged and washed with anhydrous ethanol, and then dried in a vacuum drying oven at 100℃ to prepare NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3O2@Cu-DABCO / PTA.
[0070] The prepared NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2@Cu-DABCO / PTA is used as the positive electrode active material, and is added to N-methylpyrrolidone with a binder polyvinylidene fluoride (PVDF) and a conductive agent CNT (CNT concentration is 15 wt%) for slurry. Based on the total weight of the slurry, the content of the positive electrode active material is 85 wt%, the content of the binder is 7.5 wt%, and the content of the conductive agent is 7.5 wt%. The positive electrode slurry is evenly coated on aluminum foil, then baked and dried at 110°C, and cooled to obtain a positive electrode sheet. The prepared positive electrode sheet is matched with a hard carbon negative electrode, and the electrolyte is a conventional carbonate electrolyte to assemble a full battery.
[0071] Example 2
[0072] 1g of NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2 (O3 type structure, the second metal element includes Ni, Fe and Mn) is dispersed in 60ml N,N-dimethylformamide, stirred and ultrasonicated to obtain a suspension. 22mg Cu(NO3)2 (first metal source), 20mg trimesic acid (BTC, first organic ligand), 30mg triethylenediamine (DABCO, second organic ligand) are added to the above suspension, stirred for 30min and ultrasonicated for 30min, wherein the weight ratio of layered oxide: first metal source: first organic ligand: second organic ligand is 1000:22:20:30, and the amount of solvent used is 60mL relative to 1g of layered oxide. The suspension is then transferred to a tetrafluoroethylene solvent thermal reactor, and the solvent thermal reactor is placed in a muffle furnace for solvent thermal reaction, the reaction temperature is 150℃, and the reaction time is 12h. After the reaction, the suspension is centrifuged and washed with anhydrous ethanol, and then dried in a vacuum drying oven at 100℃, i.e. NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2@Cu-DABCO / BTC.
[0073] The prepared NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3O2@Cu-DABCO / BTC is used as the positive electrode active material, and is added to N-methylpyrrolidone with a binder polyvinylidene fluoride (PVDF) and a conductive agent CNT-15% for slurry. Based on the total weight of the slurry, the content of the positive electrode active material is 85% by weight, the content of the binder is 7.5% by weight, and the content of the conductive agent is 7.5% by weight; the positive electrode slurry is evenly coated on aluminum foil, then baked and dried at 110°C, and the positive electrode sheet is obtained after cooling. The prepared positive electrode sheet is matched with a hard carbon negative electrode, and the electrolyte is a conventional carbonate electrolyte to assemble a full battery.
[0074] Example 3
[0075] 1gNaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2 (O3 type structure, the second metal element includes Ni, Fe and Mn) is dispersed in 60ml N,N-dimethylformamide, stirred and ultrasonicated to obtain a suspension. 22mg Zn(NO3)2 (first metal source), 30mg terephthalic acid (PTA, first organic ligand), 30mg triethylenediamine (DABCO, second organic ligand) are added to the above suspension, stirred for 30min and ultrasonicated for 30min, wherein the weight ratio of layered oxide: first metal source: first organic ligand: second organic ligand is 1000:22:30:30, and the amount of solvent is 60mL relative to 1g of layered oxide. The suspension is then transferred to a tetrafluoroethylene solvent thermal reactor, and the solvent thermal reactor is placed in a muffle furnace for solvent thermal reaction, the reaction temperature is 150℃, and the reaction time is 12h. After the reaction, the suspension is centrifuged and washed with anhydrous ethanol, and then dried in a vacuum drying oven at 100℃, i.e. NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2@Zn-DABCO / PTA.
[0076] The prepared NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2@Zn-DABCO / PTA is used as the positive electrode active material, and is added to N-methylpyrrolidone with a binder polyvinylidene fluoride (PVDF) and a conductive agent CNT-15% for slurry. Based on the total weight of the slurry, the content of the positive electrode active material is 85% by weight, the content of the binder is 7.5% by weight, and the content of the conductive agent is 7.5% by weight; the positive electrode slurry is evenly coated on aluminum foil, then baked and dried at 110°C, and the positive electrode sheet is obtained after cooling. The prepared positive electrode sheet is matched with a hard carbon negative electrode, and the electrolyte is a conventional carbonate electrolyte to assemble a full battery.
[0077] Example 4
[0078] In this embodiment, the positive electrode material and the full battery are prepared according to the method in Example 1. The difference from Example 1 is that the raw materials are added in a ratio of 1000:0.05:0.15:0.15, which is the weight ratio of layered oxide: first metal source: first organic ligand: second organic ligand. The rest of the process is the same as Example 1.
[0079] Example 5
[0080] In this embodiment, the positive electrode material and the full battery are prepared according to the method in Example 1. The difference from Example 1 is that the raw materials are added in a ratio of 1000:70:84:84, which is the weight ratio of layered oxide: first metal source: first organic ligand: second organic ligand. The rest of the process is the same as Example 1.
[0081] Example 6
[0082] In this embodiment, the positive electrode material and the full battery are prepared according to the method in Example 1. The difference from Example 1 is that the raw materials are added in a weight ratio of 1000:220:300:300 of layered oxide: first metal source: first organic ligand: second organic ligand, and the rest of the process is the same as Example 1.
[0083] Example 7
[0084] In this embodiment, the positive electrode material and the full battery are prepared according to the method in Example 1. The difference from Example 1 is that the second organic ligand triethylenediamine (DABCO) is replaced by 2-methyl-1,4-diazidebicyclo[2.2.2]octane (i.e., in the compound structure shown in formula (1), R1 is methyl and R2~R6 are hydrogen). The rest of the process is the same as in Example 1.
[0085] Example 8
[0086] In this embodiment, the positive electrode material and the full battery are prepared according to the method in Example 1. The difference from Example 1 is that the weight ratio of layered oxide: first metal source: first organic ligand: second organic ligand is 1000:2:19:19, and the rest of the process is the same as Example 1.
[0087] Comparative Example 1
[0088] Ni without MOF coating 1 / 3 Fe 1 / 3 Mn 1 / 3O2 is used as the positive electrode active material, and is added to N-methylpyrrolidone with a binder polyvinylidene fluoride (PVDF) and a conductive agent CNT-15% by weight for slurry. Based on the total weight of the slurry, the content of the positive electrode active material is 85% by weight, the content of the binder is 7.5% by weight, and the content of the conductive agent is 7.5% by weight; the positive electrode slurry is evenly coated on aluminum foil, then baked and dried at 110°C, and cooled to obtain a positive electrode sheet. The prepared positive electrode sheet is matched with a hard carbon negative electrode to assemble a full battery.
[0089] Comparative Example 2
[0090] This comparative example refers to the preparation method in Example 1, which is different from Example 1 in that the second organic ligand DABCO is not added, and comprises the following steps:
[0091] 1g of NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2 was dispersed in 60 ml of N,N-dimethylformamide, stirred and ultrasonicated to obtain a suspension. 22 mg of Cu(NO3)2 and 60 mg of trimesic acid (BTC) were added to the above suspension, stirred for 30 min and ultrasonicated for 30 min. The suspension was then transferred to a tetrafluoroethylene solvent thermal reactor, and the solvent thermal reactor was placed in a muffle furnace for solvent thermal reaction at a reaction temperature of 150 ° C and a reaction time of 12 h. After the reaction, the suspension was centrifuged and washed with anhydrous ethanol, and then dried in a vacuum drying oven at 100 ° C, i.e., NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2@Cu-BTC.
[0092] The prepared NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2@Cu-BTC is used as the positive electrode active material, and the binder polyvinylidene fluoride (PVDF) and the conductive agent CNT-15% are added to N-methylpyrrolidone for slurry. Based on the total weight of the slurry, the content of the positive electrode active material is 85% by weight, the content of the binder is 7.5% by weight, and the content of the conductive agent is 7.5% by weight; the positive electrode slurry is evenly coated on aluminum foil, then baked and dried at 110°C, and the positive electrode sheet is obtained after cooling. The prepared positive electrode sheet is matched with the hard carbon negative electrode to assemble into a full battery.
[0093] In order to achieve better coordination effect of preparing MOF material and coating effect of MOF material coating layer as much as possible, in the above embodiments, some raw materials are added in excess, specifically: in the layered oxide, the first metal source, the first organic ligand and the second organic ligand forming the positive electrode material, the first metal source, the first organic ligand and the second organic ligand are added in excess; in the first metal source, the first organic ligand and the second organic ligand forming the MOF material, the first organic ligand and the second organic ligand are added in excess based on the complete conversion of the first metal element in the first metal source into the MOF material; the actual component contents of the positive electrode material and the MOF coating layer prepared in the embodiments are listed in Table 1.
[0094] The component contents and structural parameters of the positive electrode materials prepared in the above examples and comparative examples are listed in the following Table 1.
[0095] Table 1
[0096]
[0097] In Table 1, the data marked with “*” are based on the total weight of the positive electrode material, and the data marked with “**” are based on the total weight of the MOF material coating layer.
[0098] Test Case
[0099] The soft-pack batteries assembled from the above embodiments and comparative examples were subjected to charge and discharge cycle tests, including room temperature cycles.
[0100] Normal temperature cycle: The whole battery was clamped and mounted on the test instrument, placed in an environment of 25±2℃, with a cycle rate of 1C and a voltage window of 2.0~4.1V. The capacity retention rate during 500 cycles was recorded, and the battery volume at 100 cycles was measured by the drainage method. After 500 cycles, the gas in the battery was removed with a syringe, and the gas composition was determined by a gas chromatograph-mass spectrometer. The test results are listed in Table 2 below.
[0101] Table 2
[0102]
[0103] According to the data in Tables 1 and 2 above, we can see that:
[0104] Tm-DABCO coating was introduced into the coating layer of the positive electrode materials prepared in Examples 1 to 8, no coating was performed in Comparative Example 1, and Tm-BTC coating was performed in Comparative Example 2 but DABCO or its derivatives were not introduced.
[0105] From the aspect of coating thickness, Example 6 was over-coated, and the coating thickness reached 3.57 μm; the thickness of the coating in Examples 1 to 5 and 7 to 8 was within the optimized thickness range (0.1 to 3 μm) provided in the present disclosure. Compared with the positive electrode material in Example 6, the positive electrode materials in Examples 1 to 5 and 7 to 8 can obtain higher first charge capacity, first discharge capacity and first efficiency; this is because the excessively thick coating in Example 6 caused a larger impedance, which hindered the capacity; in addition, the coating obtained by synthesizing using the preferred ratio (Examples 1 to 3, 7) had a thickness of about 0.4 μm, and the coating thickness had good consistency.
[0106] Compared with the uncoated comparative example 1, the Tm-BTC coated comparative example 2 has a higher capacity retention rate and better cycle stability, and the gas production volume is significantly reduced, indicating that the coating layer inhibits the side reactions in the battery cell, improves the material stability during the cycle, and reduces the gas production while improving the cycle life. The proportion of oxidizing CO2 in the gas types in comparative example 2 is significantly reduced, indicating that the introduced coating layer acts on the positive electrode and has the effect of reducing the side reactions at the interface of the positive electrode material.
[0107] On the basis of Comparative Example 2, Examples 1 to 8 introduce DABCO or its derivatives as ligands of the MOF coating layer, which can further improve the capacity retention rate of the battery cell and reduce the volume of gas production, and can further reduce the proportion of oxidizing gas CO2. This shows that DABCO and its derivatives have an additional inhibitory effect on the side reactions of the battery cell, which comes from the reaction between DABCO and its derivatives and active oxygen. DABCO and its derivatives can effectively absorb and bind the active oxygen generated by the positive electrode material, thereby preventing it from having side reactions with the electrolyte.
[0108] Furthermore, when comparing Examples 1 to 5, 7 to 8 with Example 6, the coating layer in Example 6 is too thick, and the content of the MOF coating layer in the positive electrode material is relatively high, which can also reduce the interface side reaction of the positive electrode material and reduce the gas volume, and the effect is equivalent to that of other Examples (Examples 1 to 5, 7 to 8), indicating that the overly thick coating layer cannot bring additional inhibitory effects. In terms of comprehensive battery cycle stability, the introduction of an overly thick coating layer cannot comprehensively improve the performance of the battery.
[0109] Comparing Examples 1 to 3 and 7 with Example 4, the content of the MOF material coating layer in Examples 1 to 3 is within the preferred content range provided in the present disclosure, and the content of the MOF material coating layer in Example 4 is lower. Compared with the positive electrode material in Example 4, the positive electrode materials prepared in Examples 1 to 3 and 7 have a higher first effect, and the gas production volume after 500 cycles and the CO2 content in the produced gas are lower; Comparing Examples 1 to 3 and 7 with Example 5, the content of the MOF material coating layer in Examples 1 to 3 and 7 is within the preferred content range provided in the present disclosure, and the content of the MOF material coating layer in Example 5 is higher. Compared with the positive electrode material in Example 5, the positive electrode materials prepared in Examples 1 to 3 and 7 have a higher battery specific capacity and first effect; It shows that the positive electrode materials with preferred component contents in Examples 1 to 3 and 7 of the present disclosure have better comprehensive performance;
[0110] Comparing Examples 1 to 3 and 7 with Example 8, the component contents of the MOF coating layers in Examples 1 to 3 and 7 are within the preferred range, and the battery performance of the positive electrode materials prepared in Examples 1 to 3 and 7 is equivalent to that in Example 8, but the positive electrode materials in Examples 1 to 3 and 7 have a higher 500-cycle capacity retention rate and a lower gas production volume and CO2 content in the produced gas.
[0111] The preferred embodiments of the present disclosure are described in detail above; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0112] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0113] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A positive electrode material for a sodium ion battery, characterized in that: It includes a layered oxide as the core and a MOF material coating layer coated on the surface of the layered oxide; the MOF material coating layer includes a first metal coordination compound, and the organic ligand in the first metal coordination compound includes a first organic ligand and a second organic ligand. The first organic ligand is selected from one or more of isophthalic acid, phthalic acid, terephthalic acid, trimellitic acid, 1,2,4-benzenetricarboxylic acid, and 1,3,5-benzenetricarboxylic acid; the second organic ligand includes a compound having the structure shown in the following formula (1): Formula (1); wherein R1 to R6 are the same or different and are independently selected from one of hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkenyl group having 1 to 10 carbon atoms or an alkynyl group having 1 to 10 carbon atoms; The layered oxide includes a compound having the composition shown in the following formula (2): Na x TmO2 formula (2); wherein Tm is a second metal element, and Tm is selected from one or more of Cu, Fe, Mn, Ca, Ni, Co, Cr, Zn, Ti, V, Zr, Mg, Al, Li and Nb, 0 <x≤1; The thickness of the MOF material coating layer is 0.35 - 2.89 μm.
2. The positive electrode material according to claim 1, characterized in that The first metal element in the first metal coordination compound is selected from one or more of Cu, Fe, Mn, Ca, Ni, Co, Cr, Zn, Ti, V, Zr, Mg, Al, Li, and Nb; In formula (1), R1 - R6 are the same or different and are each independently selected from one of hydrogen, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, vinyl, propenyl, allyl, butenyl, butadienyl, ethynyl, propargyl, and butynyl; The structure of the layered oxide is selected from one or more of P2 type, O3 type, P3 type, and tunnel type; 3. The positive electrode material according to claim 2, characterized in that Based on the total weight of the positive electrode material, the content of the layered oxide is 58 - 99.9% by weight, and the content of the MOF material coating layer is 0.1 - 42% by weight; Based on the total weight of the MOF material coating layer, the content of the first metal element is 5 - 50% by weight, the content of the first organic ligand is 15 - 60% by weight, and the content of the second organic ligand is 15 - 60% by weight.
4. The positive electrode material according to claim 1, characterized in that The particle size of the positive electrode material is 2.1 - 23 μm; the particle size of the layered oxide is 2 - 20 μm.
5. A method for preparing a positive electrode material for a sodium ion battery, characterized in that: It includes the following steps: Making the layered oxide, the first metal source, and the organic ligand contact and react in a solvent; wherein the organic ligand includes a first organic ligand and a second organic ligand. The first organic ligand is selected from one or more of isophthalic acid, phthalic acid, terephthalic acid, trimellitic acid, 1,2,4-benzenetricarboxylic acid, and 1,3,5-benzenetricarboxylic acid; the second organic ligand is a compound having the structure shown in the following formula (1): Formula (1); wherein R1 to R6 are the same or different and are independently selected from one of hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkenyl group having 1 to 10 carbon atoms and an alkynyl group having 1 to 10 carbon atoms; The layered oxide includes a compound having the composition shown in the following formula (2): Na x TmO2 formula (2); wherein Tm is a second metal element, and Tm is selected from one or more of Cu, Fe, Mn, Ca, Ni, Co, Cr, Zn, Ti, V, Zr, Mg, Al, Li and Nb, 0 <x≤1; The weight ratio of the layered oxide : the first metal source : the first organic ligand : the second organic ligand is 1000 : 2 - 70 : 30 - 84 : 30 - 84.
6. The method according to claim 5, characterized in that The first metal source is selected from one or more of nitrates, sulfates, halide salts, and phosphates of the first metal element; the first metal element is selected from one or more of Cu, Fe, Mn, Ca, Ni, Co, Cr, Zn, Ti, V, Zr, Mg, Al, Li, and Nb; The structure of the layered oxide is selected from one or more of P2 type, O3 type, P3 type, and tunnel type, 0 < x ≤ 1; the particle size of the layered oxide is 2 - 20 μm; In formula (1), R1 to R6 are the same or different and are independently selected from one of hydrogen, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, vinyl, propenyl, allyl, butylene, butadienyl, ethynyl, propargyl and butylene; The solvent is selected from one or more of acetonitrile, ethanol, ethylene glycol, methanol, propanol, tetrahydrofuran and N, N-dimethylformamide.
7. The method according to claim 5, characterized in that The contact reaction conditions include: in a solvent thermal reactor, the reaction temperature is 100-300° C., and the reaction time is 5-36 hours.
8. The positive electrode material prepared according to the method according to any one of claims 5 to 7.
9. A positive electrode sheet for a sodium ion battery, comprising the positive electrode material according to any one of claims 1 to 4 and 8.
10. A sodium ion battery comprising the positive electrode sheet according to claim 9.
Citation Information
Patent Citations
Positive plate and application thereof
CN115692622A
Glassy-state metal organic framework material modified ternary positive electrode material and preparation method and application thereof
CN117894971A