A method for purifying natural graphite based on molten alkali salt mixture
Through the combined treatment of molten alkali salt mixture and acid solution, the purification process of natural graphite is simplified, the problems of complex process and high energy consumption in the prior art are solved, and high efficiency and low cost high-purity graphite purification is achieved.
Patent Information
- Application Number
- CN202411070834.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-06
AI Technical Summary
The existing natural graphite purification process is complex, has high energy consumption and is expensive, making it difficult to achieve efficient purification.
The molten alkali salt mixture is used for calcination and melting treatment, combined with the acid solution soaking and cleaning treatment, and the impurities in the graphite are converted and removed through the combination of alkali and borate to improve the purity of graphite.
The process flow is simplified, energy consumption is reduced, purification efficiency is improved, and high-purity natural graphite is obtained, with a purity of more than 99.9%, which is suitable for large-scale industrial production.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of natural graphite purification, and in particular relates to a method for purifying natural graphite based on a molten alkali salt mixture. Background Art
[0002] High-purity graphite is widely used in industry and life. For example, the negative electrode of lithium-ion batteries requires a graphite purity of more than 99.95%. However, after mining and flotation, the purity of natural graphite ore is often around 90%, which is difficult to use directly. Therefore, it is of great significance to develop natural graphite purification technology.
[0003] At present, the main methods for purifying natural graphite are mixed acid method, high temperature calcination method and alkaline acid method. The mixed acid method requires acid treatment under high temperature conditions and requires the use of a mixture of hydrofluoric acid, sulfuric acid and hydrochloric acid. The volatilization of a large amount of high-concentration acid during operation, its strong corrosiveness and safety limit its large-scale application. The high-temperature calcination method usually requires calcination and purification at a high temperature of about 3000°C, with high energy consumption and large equipment investment during the purification process. As a mature process for graphite purification, the alkaline acid method is relatively complicated in operation but has significant effects. The alkaline acid method mainly removes impurities in graphite and improves the purity of graphite by combining alkaline substances (such as sodium hydroxide or potassium hydroxide) and oxidants (such as concentrated nitric acid, concentrated sulfuric acid or concentrated hydrochloric acid).
[0004] The commonly used alkali-acid purification process is divided into two steps, one is alkali treatment and the other is acid treatment. In order to improve the purification effect, most of them tend to use the two-step alkali-acid combined method. For example, the Chinese patent with publication number CN116692850A and invention name "A green purification method for natural graphite" adopts the "alkali roasting-primary acid treatment-secondary acid treatment" method to purify graphite; and the Chinese patent with publication number CN103449425A and invention name "A method for purifying high-carbon natural flake graphite to prepare high-purity graphite by alkali acid-complexation method" adopts the "alkali roasting-aqua regia acid treatment-alkali treatment-cooperative acid treatment" process to purify graphite. This multi-step combined treatment process can indeed effectively improve the purity. However, more steps also mean that the preparation process is complicated, the purification process is long, more equipment is used and the cost is high. Summary of the invention
[0005] The purpose of the present invention is to provide a method for purifying natural graphite based on a molten alkali salt mixture, so as to solve the problem of complex preparation process in the prior art.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The present invention provides a method for purifying natural graphite based on a molten alkali salt mixture, comprising the following steps:
[0008] S1: mixing natural graphite with an alkali salt mixture, and then calcining and melting the mixture to obtain a first intermediate product;
[0009] S2: soaking the first intermediate product in an acid solution to obtain a second intermediate product;
[0010] S3: washing, filtering and drying the second intermediate product in sequence to obtain purified natural graphite;
[0011] The alkali salt mixture consists of an alkali and a mixed salt, the alkali is sodium hydroxide or lithium hydroxide, the mixed salt consists of a first component and a second component, the first component is at least one of sodium fluoride, sodium chloride and lithium fluoride, and the second component is at least one of sodium metaborate, sodium borate, lithium metaborate and lithium borate.
[0012] In the specific implementation process, the mass ratio of the natural graphite to the alkali salt mixture is 1:(0.1~1).
[0013] In the specific implementation process, the mass ratio of alkali in the alkali salt mixture to natural graphite is (4-80):100; the mass ratio of mixed salt in the alkali salt mixture to natural graphite is (6-35):100; the mass ratio of the first component to the second component in the mixed salt is 1:(1-3).
[0014] In the specific implementation process, in S1, calcination and melting treatment is carried out at a temperature of 500°C to 1000°C; the time of calcination and melting treatment is 0.5h to 6h.
[0015] In a specific implementation process, the acid solution is one of a sulfuric acid solution, a hydrochloric acid solution and a nitric acid solution.
[0016] In the specific implementation process, the mass fraction of the acid solution is 5%~20%.
[0017] In the specific implementation process, the usage ratio of the natural graphite to the acid solution is 1g: (2.5~10)mL.
[0018] In the specific implementation process, in S2, the immersion is carried out at a temperature of 25°C to 45°C; the immersion time is 0.5h to 6h.
[0019] In the specific implementation process, the cleaning is carried out in sequence using a sodium pyrophosphate solution and deionized water; the cleaning temperature of the sodium pyrophosphate solution is 25°C to 60°C; the dosage ratio of the natural graphite to the sodium pyrophosphate solution is 1g: (2.5~10)mL, wherein the concentration of the sodium pyrophosphate solution is 5g / L~20g / L; the cleaning temperature of the deionized water is 25°C to 60°C;
[0020] The temperature of the drying process is 60° C. to 120° C., and the time of the drying process is 1 h to 6 h.
[0021] In the specific implementation process, the type of natural graphite is natural spherical graphite or natural flake graphite.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] The present invention provides a method for purifying natural graphite based on a molten alkali salt mixture, wherein the method firstly calcines and melts the natural graphite and the alkali salt mixture under high temperature conditions, effectively and quickly converts the inorganic impurities in the natural graphite into acid-soluble substances by regulating the alkali treatment environment, and then removes the acid-soluble substances during the acid leaching process. The alkali in the alkali salt mixture converts the difficult-to-remove silicon and aluminum in the natural graphite into sodium silicate and aluminum silicate, and other trace impurities such as iron, calcium, magnesium, etc. are also converted into hydroxides under an alkaline environment; the mixed salt in the alkali salt mixture is composed of a first component and a second component, the first component selects at least one of sodium fluoride, sodium chloride and lithium fluoride, and can convert part of the impurities into halides, and the second component selects at least one of sodium metaborate, sodium borate, lithium metaborate and lithium borate as a flux, which plays an important role in the system. Specifically, the borate or metaborate used in the second component can accelerate the reaction of metal ions, and during the calcination and melting process, react with metal ions to generate substances that are easily soluble under acidic conditions, thereby effectively purifying the graphite, and can also promote the first component to react with impurities in the graphite to generate substances that are easy to pickle, further purifying the graphite. In summary, the present invention optimizes the existing purification route and improves the purification efficiency by developing a more effective alkali treatment process and formula.
[0024] The present invention provides a method for purifying natural graphite based on a molten alkali salt mixture, wherein the method mainly uses an alkali salt mixture for purification, and by optimizing the components and proportions of the alkali salt mixture, an efficient and accurate purification process is achieved, and the purified natural graphite has a high degree of consistency, and can purify natural graphite originally having a purity of 90% to more than 99.9%, showing an extremely high purification effect. At the same time, the purification method provided by the present invention is simple and easy to operate, has low processing cost, and high purification efficiency, and is very suitable for large-scale industrial preparation and purification of natural graphite.
[0025] Furthermore, the present invention also introduces sodium pyrophosphate solution as an auxiliary cleaning means, which is specifically used to remove sol-like impurities and improve cleaning efficiency. DETAILED DESCRIPTION
[0026] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0027] In this article, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0028] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0029] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0030] The invention provides a method for purifying natural graphite based on a molten alkali salt mixture. The method comprises the following steps: firstly mixing natural graphite and an alkali salt mixture together in a solid state, and then calcining and melting the mixture to obtain a first intermediate product; then immersing the first intermediate product in an acid solution to obtain a second intermediate product; and finally sequentially washing, filtering and drying the obtained second intermediate product to obtain purified natural graphite, wherein the purity of the purified natural graphite is above 99.9%.
[0031] The above method for purifying natural graphite based on molten alkali salt mixture comprises the following specific steps:
[0032] S1: Mix natural graphite and an alkali salt mixture in a mass ratio of 1:(0.1~1), and then calcine and melt them at a temperature of 500℃~1000℃ for 0.5h~6h to obtain a first intermediate product; wherein the alkali salt mixture consists of an alkali and a mixed salt, the alkali is sodium hydroxide or lithium hydroxide, the mixed salt consists of a first component and a second component, the first component is at least one of sodium fluoride, sodium chloride and lithium fluoride, and the second component is at least one of sodium metaborate, sodium borate, lithium metaborate and lithium borate.
[0033] The invention of the present invention mainly lies in the design of the alkali treatment formula. The alkali in the alkali salt mixture used for alkali treatment, such as sodium hydroxide and lithium hydroxide, can promote the conversion of silicon and aluminum that are difficult to remove in natural graphite into sodium silicate and aluminum silicate. Other trace impurities such as iron, calcium and magnesium can also be converted into hydroxides under alkaline conditions. The first component of the mixed salt in the alkali salt mixture can convert part of the impurities into halides during calcination and melting treatment. For example, chloride salts can convert part of the impurities into chlorides during calcination, and fluoride salts can convert part of the impurities into fluorides during calcination. The second component of the mixed salt in the alkali salt mixture, namely borates and metaborates, acts as a flux during the treatment process. The specific functions of the second component include: accelerating the reaction of metal ions and increasing the reaction rate; reacting with metal ions during calcination and melting treatment to generate substances that are easily soluble under acidic conditions, which helps to purify graphite; promoting the reaction of the first component with impurities in graphite to generate substances that are easy to pickle, further realizing the purification of graphite.
[0034] The above formula combination can effectively remove impurities in natural graphite, thereby improving the purification effect and optimizing the existing purification route.
[0035] Specifically, the mass ratio of alkali in the alkali salt mixture to natural graphite is (4-80):100, the mass ratio of mixed salt in the alkali salt mixture to natural graphite is (6-35):100; the mass ratio of the first component to the second component in the mixed salt is 1:(1-3).
[0036] S2: Soak the first intermediate product in an acid solution at a temperature of 25°C to 45°C for 0.5h to 6h to obtain a second intermediate product; wherein the acid solution is one of a sulfuric acid solution, a hydrochloric acid solution and a nitric acid solution, and the mass fraction of the acid solution is 5% to 20%; the dosage ratio of natural graphite to the acid solution is 1g: (2.5~10)mL.
[0037] S3: The second intermediate product is sequentially washed, filtered and dried to obtain purified natural graphite, wherein the washing is sequentially carried out with a sodium pyrophosphate solution and deionized water, and the sodium pyrophosphate solution is used to remove sol impurities.
[0038] Specifically, when sodium pyrophosphate solution is used for cleaning, the cleaning temperature of the sodium pyrophosphate solution is 25°C to 60°C, the usage ratio of natural graphite to sodium pyrophosphate solution is 1g: (2.5~10)mL, wherein the concentration of the sodium pyrophosphate solution is 5g / L to 20g / L. When deionized water is used for cleaning, the cleaning temperature of the deionized water is 25°C to 60°C.
[0039] The drying process is carried out in a common oven, the drying temperature is 60°C to 120°C, and the drying time is 1h to 6h.
[0040] The type of natural graphite in the above purification method is natural spherical graphite or natural flake graphite.
[0041] The method for purifying natural graphite based on a molten alkali salt mixture provided by the invention is suitable for purifying natural spherical graphite and natural flake graphite.
[0042] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0043] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0044] The present invention is further described in detail below in conjunction with specific embodiments, which are intended to explain the present invention rather than to limit it.
[0045] Example 1
[0046] 100 g of natural flake graphite was mixed with 100 g of an alkali salt mixture (in terms of mass percentage, the alkali salt mixture consisted of 80% sodium hydroxide, 10% sodium chloride and 10% sodium borate), and then calcined and melted at 500° C. for 6 hours to obtain a first intermediate product; the first intermediate product was then placed in 500 mL of a 10% sulfuric acid solution and soaked at 45° C. for 2 hours to obtain a second intermediate product; the second intermediate product was washed with 500 mL of a sodium pyrophosphate solution (with a concentration of 5 g / L) at 25° C., and then washed with deionized water at 25° C. until the second intermediate product was neutral, filtered to obtain a filter cake, and then the filter cake was dried at 60° C. for 6 hours to obtain purified natural flake graphite.
[0047] In the calcination experiment test, 2g of purified natural flake graphite was accurately weighed and placed in a porcelain boat with constant weight, and the mass of the purified natural flake graphite and the porcelain boat was recorded; the porcelain boat was placed in a muffle furnace that had been heated to 900℃~1000℃, and after preheating for 1min, it was pushed into the high temperature zone and burned with air flow until there were no black spots; the porcelain boat was taken out and placed in a dryer after cooling slightly, cooled to room temperature, and weighed. By comparing the mass change of the substance in the porcelain boat before and after burning, the mass percentage of ash was calculated, and then the purity of the purified natural flake graphite was obtained.
[0048] According to the above calcination experiment test, the purity of the purified natural flake graphite obtained in this embodiment is 99.95%.
[0049] Example 2
[0050] 100g of natural flake graphite is mixed with 10g of an alkali salt mixture (in terms of mass percentage, the alkali salt mixture consists of 40% sodium hydroxide, 10% sodium fluoride, 20% sodium chloride and 30% lithium borate), and then calcined and melted at 1000°C for 0.5h to obtain a first intermediate product; the first intermediate product is then placed in 250mL of a 20% hydrochloric acid solution and soaked at 25°C for 6h to obtain a second intermediate product; the second intermediate product is washed with 250mL of a sodium pyrophosphate solution (concentration of 20g / L) at 60°C, and then washed with deionized water at 25°C until the second intermediate product is neutral, filtered to obtain a filter cake, and then the filter cake is dried at 80°C for 6h to obtain purified natural flake graphite.
[0051] In the calcination experiment test, 2g of purified natural flake graphite was accurately weighed and placed in a porcelain boat with constant weight, and the mass of the purified natural flake graphite and the porcelain boat was recorded; the porcelain boat was placed in a muffle furnace that had been heated to 900℃~1000℃, and after preheating for 1min, it was pushed into the high temperature zone and burned with air flow until there were no black spots; the porcelain boat was taken out and placed in a dryer after cooling slightly, cooled to room temperature, and weighed. By comparing the mass change of the substance in the porcelain boat before and after burning, the mass percentage of ash was calculated, and then the purity of the purified natural flake graphite was obtained.
[0052] According to the above calcination experiment test, the purity of the purified natural flake graphite obtained in this embodiment is 99.96%.
[0053] Example 3
[0054] 100g of natural spherical graphite is mixed with 20g of an alkali salt mixture (in terms of mass percentage, the alkali salt mixture consists of 40% sodium hydroxide, 15% lithium fluoride, 40% sodium borate and 5% lithium metaborate), and then calcined and melted at 800°C for 1h to obtain a first intermediate product; then the first intermediate product is placed in 1000mL of a 5% nitric acid solution and soaked at 45°C for 6h to obtain a second intermediate product; the second intermediate product is washed with 1000mL of a sodium pyrophosphate solution (with a concentration of 15g / L) at 45°C, and then washed with deionized water at 60°C until the second intermediate product is neutral, filtered to obtain a filter cake, and then the filter cake is dried at 120°C for 1h to obtain purified natural spherical graphite.
[0055] In the calcination experiment test, 2g of purified natural spherical graphite was accurately weighed and placed in a porcelain boat with constant weight, and the mass of the purified natural spherical graphite and the porcelain boat was recorded; the porcelain boat was placed in a muffle furnace that had been heated to 900℃~1000℃, and after preheating for 1min, it was pushed into the high temperature zone and burned with air flow until there were no black spots; the porcelain boat was taken out and placed in a dryer after cooling slightly, cooled to room temperature, and weighed. By comparing the mass change of the substance in the porcelain boat before and after burning, the mass percentage of ash was calculated, and then the purity of the purified natural spherical graphite was obtained.
[0056] According to the above calcination test, the purity of the purified natural spherical graphite obtained in this embodiment is 99.94%.
[0057] Example 4
[0058] 100g of natural spherical graphite is mixed with 40g of an alkali salt mixture (in terms of mass percentage, the alkali salt mixture consists of 40% sodium hydroxide, 40% sodium borate and 20% sodium chloride), and then calcined and melted at 700°C for 0.5h to obtain a first intermediate product; the first intermediate product is then placed in 800mL of a 10% sulfuric acid solution and soaked at 45°C for 3h to obtain a second intermediate product; the second intermediate product is washed with 800mL of a sodium pyrophosphate solution (with a concentration of 10g / L) at 45°C, and then washed with deionized water at 60°C until the second intermediate product is neutral, filtered to obtain a filter cake, and then the filter cake is dried at 90°C for 3h to obtain purified natural spherical graphite.
[0059] In the calcination experiment test, 2g of purified natural spherical graphite was accurately weighed and placed in a porcelain boat with constant weight, and the mass of the purified natural spherical graphite and the porcelain boat was recorded; the porcelain boat was placed in a muffle furnace that had been heated to 900℃~1000℃, and after preheating for 1min, it was pushed into the high temperature zone and burned with air flow until there were no black spots; the porcelain boat was taken out and placed in a dryer after cooling slightly, cooled to room temperature, and weighed. By comparing the mass change of the substance in the porcelain boat before and after burning, the mass percentage of ash was calculated, and then the purity of the purified natural spherical graphite was obtained.
[0060] According to the above calcination test, the purity of the purified natural spherical graphite obtained in this embodiment is 99.96%.
[0061] Example 5
[0062] 100g of natural flake graphite is mixed with 50g of an alkali salt mixture (in terms of mass percentage, the alkali salt mixture consists of 30% lithium hydroxide, 30% sodium fluoride and 40% sodium metaborate), and then calcined and melted at 800°C for 3h to obtain a first intermediate product; the first intermediate product is then placed in 1000mL of a 10% sulfuric acid solution and soaked at 45°C for 0.5h to obtain a second intermediate product; the second intermediate product is washed with 1000mL of a sodium pyrophosphate solution (with a concentration of 5g / L) at 25°C, and then washed with deionized water at 60°C until the second intermediate product is neutral, filtered to obtain a filter cake, and then the filter cake is dried at 90°C for 4h to obtain purified natural flake graphite.
[0063] In the calcination experiment test, 2g of purified natural flake graphite was accurately weighed and placed in a porcelain boat with constant weight, and the mass of the purified natural flake graphite and the porcelain boat was recorded; the porcelain boat was placed in a muffle furnace that had been heated to 900℃~1000℃, and after preheating for 1min, it was pushed into the high temperature zone and burned with air flow until there were no black spots; the porcelain boat was taken out and placed in a dryer after cooling slightly, cooled to room temperature, and weighed. By comparing the mass change of the substance in the porcelain boat before and after burning, the mass percentage of ash was calculated, and then the purity of the purified natural flake graphite was obtained.
[0064] According to the above calcination experiment test, the purity of the purified natural flake graphite obtained in this embodiment is 99.98%.
[0065] In summary, the method for purifying natural graphite based on a molten alkali salt mixture provided by the present invention simplifies the process flow of the traditional purification method, reduces energy consumption, and improves the processing efficiency and the purity of natural graphite, and can obtain natural graphite with a purity of more than 99.9%.
[0066] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A method for purifying natural graphite based on a molten alkali salt mixture, It is characterized in that The following steps are involved: S1: mixing natural graphite with an alkali salt mixture, and then calcining and melting the mixture to obtain a first intermediate product; S2: soaking the first intermediate product in an acid solution to obtain a second intermediate product; S3: washing, filtering and drying the second intermediate product in sequence to obtain purified natural graphite; The alkali salt mixture is composed of an alkali and a mixed salt, the alkali is sodium hydroxide or lithium hydroxide, the mixed salt is composed of a first component and a second component, the first component is at least one of sodium fluoride, sodium chloride and lithium fluoride, and the second component is at least one of sodium metaborate, sodium borate, lithium metaborate and lithium borate; The mass ratio of the natural graphite to the alkali salt mixture is 1:(0.1~1); The mass ratio of the alkali in the alkali salt mixture to the natural graphite is (4-80):100; the mass ratio of the mixed salt in the alkali salt mixture to the natural graphite is (6-35):100; the mass ratio of the first component to the second component in the mixed salt is 1:(1-3).
2. The method for purifying natural graphite based on a molten alkali salt mixture according to claim 1, It is characterized in that In S1, calcination and melting treatment is performed at a temperature of 500° C. to 1000° C.; the time for the calcination and melting treatment is 0.5 h to 6 h.
3. The method for purifying natural graphite based on a molten alkali salt mixture according to claim 1, It is characterized in that The acid solution is one of a sulfuric acid solution, a hydrochloric acid solution and a nitric acid solution.
4. The method for purifying natural graphite based on a molten alkali salt mixture according to claim 1, It is characterized in that The mass fraction of the acid solution is 5% to 20%.
5. The method for purifying natural graphite based on a molten alkali salt mixture according to claim 1, It is characterized in that The usage ratio of the natural graphite to the acid solution is 1 g: (2.5-10) mL.
6. The method for purifying natural graphite based on a molten alkali salt mixture according to claim 1, It is characterized in that In S2, the immersion is carried out at a temperature of 25°C to 45°C; the immersion time is 0.5h to 6h.
7. The method for purifying natural graphite based on a molten alkali salt mixture according to claim 1, It is characterized in that The cleaning is carried out in sequence by using a sodium pyrophosphate solution and deionized water; the cleaning temperature of the sodium pyrophosphate solution is 25°C to 60°C; the dosage ratio of the natural graphite to the sodium pyrophosphate solution is 1g: (2.5-10)mL, wherein the concentration of the sodium pyrophosphate solution is 5g / L to 20g / L; the cleaning temperature of the deionized water is 25°C to 60°C; The temperature of the drying process is 60° C. to 120° C., and the time of the drying process is 1 h to 6 h.
8. The method for purifying natural graphite based on a molten alkali salt mixture according to claim 1, It is characterized in that The natural graphite is natural spherical graphite or natural flake graphite.