A two-step alkali-acid purification method for natural graphite

Through the two-step alkaline-acid purification method, the repeated treatment of low-concentration sodium hydroxide and sulfuric acid solutions solves the problem of difficulty in thoroughly cleaning impurities in natural graphite, achieving high-purity and high-consistency graphite purification, and avoiding the problems of traditional methods. safety and environmental issues.

CN118579776BActive Publication Date: 2024-10-22SHAANXI HANTANG SENYUAN IND DEV GRP CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411070886.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-10-22
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

In the existing natural graphite purification method, the process of first acid treatment and then alkali treatment has the problem that impurities are difficult to thoroughly clean, resulting in poor purification effect.

Method used

A two-step alkaline-acid purification method is used. First, a low-concentration sodium hydroxide solution is used for alkali treatment to convert the impurities in the graphite into solid matter, and then a low-concentration sulfuric acid solution is used for acid treatment to remove the impurities. The purity of the graphite is improved through repeated hydrothermal reactions. and consistency.

Benefits of technology

It achieves high-purity purification of natural graphite with a purity of more than 99.9%, avoids safety issues and equipment corrosion of high-concentration alkali-acid solutions, reduces sewage treatment costs, and improves purification effects and consistency.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a two-step alkali-acid purification method for natural graphite, and belongs to the technical field of purification of natural graphite. The purification method of the invention comprises: mixing natural graphite with sodium hydroxide solution, and then performing a first hydrothermal reaction to obtain a first intermediate product; mixing the first intermediate product, sulfuric acid solution and additives, and then performing a second hydrothermal reaction to obtain a second intermediate product; mixing the second intermediate product with sodium hydroxide solution, and then performing a third hydrothermal reaction to obtain a third intermediate product; mixing the third intermediate product, sulfuric acid solution and additives, and then performing a fourth hydrothermal reaction to obtain purified natural graphite; wherein the mass fraction of the sodium hydroxide solution is 2% to 15%, and the mass fraction of the sulfuric acid solution is 5% to 10%. The invention adopts a two-step alkali-acid method for purification, which can increase the purity of natural graphite originally having a purity of 90% to 96% to more than 99.9%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of purification of natural graphite, and in particular relates to a two-step alkali-acid purification method of natural graphite. Background Art

[0002] Graphite, especially high-purity graphite, is widely used in lithium-ion battery negative electrodes, sintering molds, thermal conductive coatings, wave absorbers, semiconductors and other fields. Although natural graphite reserves are abundant, various mineral impurities inside natural graphite affect its direct use, so natural graphite must be purified.

[0003] At present, the main methods for purifying natural graphite are hydrofluoric acid method, chlorination roasting method, high-temperature purification method and alkali-acid method. Among them, the hydrofluoric acid method has high impurity removal efficiency and low energy consumption, but hydrofluoric acid is highly toxic and corrosive, and strict protective measures are required during the production process, and large environmental protection investment is required. The chlorination roasting method uses chlorine gas to react with impurities at high temperature to generate chlorides with low melting points and boiling points to escape, thereby preparing high-purity graphite, but the toxicity, strong corrosiveness and pollution of chlorine gas during operation affect practical applications. The high-temperature purification method requires heating the graphite to a high temperature of about 3000℃, so as to obtain high-purity graphite at a temperature higher than the boiling point of the impurities, but the application process has high requirements for raw materials, large investment and high energy consumption. The alkali-acid method mainly includes two steps: alkali treatment and acid treatment. After alkali-acid process treatment, most of the impurities in natural graphite can be removed, thereby improving the purity and quality of graphite.

[0004] The alkali-acid process can be further divided into two types. One is to mix graphite with alkali, and then use high-temperature roasting to convert metal impurities into solid substances such as aluminum silicate, sodium silicate, iron hydroxide, and manganese hydroxide, and then use acid to dissolve the solid substances, and obtain high-purity graphite by washing. For example, the Chinese patent with the publication number CN103449425A and the invention name "A method for preparing high-purity graphite by purifying high-carbon natural flake graphite using alkali-acid-complexation method" uses 30% alkali solution to mix with graphite, roast at a high temperature of about 700°C, and then use aqua regia to dissolve the solid substances. In order to improve the treatment effect, the technology is subsequently treated with secondary alkali and acid. However, the high-temperature roasting operation not only consumes a lot of energy, but also has uneven temperature conduction under solid conditions. Especially in mass production, the uniformity of the reaction between alkali and impurities is limited, which is not conducive to mass production of graphite with consistent purity. The other is the hydrothermal alkali-acid treatment method, specifically, graphite is hydrothermally treated with alkali or acid solution, and impurities are prompted to react with acid / alkali in a high-temperature and high-pressure aqueous solution environment. The reaction is more uniform and sufficient in the solution environment, and the hydrothermal temperature is usually within 250°C, with lower energy consumption, which has been favored by researchers and enterprises. Usually, researchers pay more attention to the hydrothermal alkali treatment process, such as the Chinese patent with the publication number CN114873592A and the invention name "A process for purifying natural graphite", which uses alkali and flux to mix with graphite, and then remove impurities at high temperature. Similarly, in order to improve the treatment effect, it adopts the acid treatment-alkali treatment-acid treatment-alkali treatment combined process, and its focus is on the preparation of the alkali treatment formula. The mass fraction of sodium hydroxide used is 16%~80%, and the flux is lithium metaborate, sodium metaborate or sodium peroxide. Its formula design is similar to the traditional high-temperature alkali roasting method. However, it is well known that silicates are poorly soluble in water. If the acid-first-then-alkali method is used, a small amount of silicates may be difficult to clean, and some impurities may still exist in the graphite after purification. Summary of the invention

[0005] The purpose of the present invention is to provide a two-step alkali-acid purification method for natural graphite, so as to solve the technical problem that impurities are difficult to be thoroughly cleaned in the purification process of the prior art using acid treatment followed by alkali treatment.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] The present invention provides a two-step alkali-acid purification method for natural graphite, comprising the following steps:

[0008] S1: mixing natural graphite with a sodium hydroxide solution, and then performing a first hydrothermal reaction to obtain a first intermediate product;

[0009] S2: mixing the first intermediate product, the sulfuric acid solution and the additive, and then performing a second hydrothermal reaction to obtain a second intermediate product;

[0010] S3: mixing the second intermediate product with a sodium hydroxide solution, and then performing a third hydrothermal reaction to obtain a third intermediate product;

[0011] S4: mixing the third intermediate product, the sulfuric acid solution and the additive, and then performing a fourth hydrothermal reaction to obtain purified natural graphite;

[0012] The mass fraction of the sodium hydroxide solution in S1 and S3 is 2% to 15%, and the mass fraction of the sulfuric acid solution in S2 and S4 is 5% to 10%.

[0013] In the specific implementation process, in S1, the usage ratio of the natural graphite to the sodium hydroxide solution is 1g: (2.5~10)mL.

[0014] In the specific implementation process, in S2, the dosage ratio of the first intermediate product to the sulfuric acid solution is 1g: (2.5~10)mL.

[0015] In the specific implementation process, in S3, the dosage ratio of the second intermediate product to the sodium hydroxide solution is 1g: (2.5~10)mL.

[0016] In the specific implementation process, in S4, the usage ratio of the third intermediate product to the sulfuric acid solution is 1 g: (2.5~10) mL.

[0017] In the specific implementation process, the additives in S2 and S4 are composed of fluoride and chloride; the mass ratio of the fluoride to the chloride is (1:16) to (3:5); the fluoride is one or both of ammonium fluoride and lithium fluoride, and the chloride is one or both of zinc chloride and lithium chloride.

[0018] In the specific implementation process, in S2, the amount of the additive is 5.5% to 9.5% of the mass of the first intermediate product; in S4, the amount of the additive is 5.5% to 9.5% of the mass of the third intermediate product.

[0019] In the specific implementation process, the reaction conditions of the first hydrothermal reaction and the third hydrothermal reaction are the same; the reaction conditions of the first hydrothermal reaction and the third hydrothermal reaction are as follows: the reaction temperature is 60°C~180°C, and the reaction time is 1h~6h.

[0020] In the specific implementation process, the reaction conditions of the second hydrothermal reaction and the fourth hydrothermal reaction are the same; the reaction conditions of the second hydrothermal reaction and the fourth hydrothermal reaction are as follows: the reaction temperature is 80°C~180°C, and the reaction time is 1h~6h.

[0021] In a specific implementation process, the type of natural graphite is natural flake graphite or natural spherical graphite.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The invention provides a two-step alkali-acid purification method for natural graphite. The method adopts a repeated two-step treatment process of first alkali and then acid to purify the natural graphite. A low-concentration sodium hydroxide solution is used for alkali treatment to convert aluminum and silicon impurities in the graphite that are difficult to treat into silicates. Subsequently, a low-concentration sulfuric acid solution is used for acid treatment to remove silicates that are difficult to clean. The acid treatment can further remove impurities such as iron and calcium in the graphite. The purification method adopts a low-concentration sodium hydroxide solution and a sulfuric acid solution for repeated alkali-acid treatment, abandons the traditional two-step hydrothermal method process of first acid and then alkali. The sodium hydroxide solution and sulfuric acid solution with lower concentrations avoid the safety problems and equipment corrosion problems of high-concentration alkali acid solutions in the process of use. Repeating the purification twice can cooperate with the low-concentration alkali acid solution to further improve the graphite purification effect. The present invention adopts the mode of first alkali treatment and then acid treatment. The alkali treatment process first performed can convert some impurities into solid substances such as aluminum silicate, sodium silicate, iron hydroxide and manganese hydroxide with the help of sodium hydroxide solution, and remove them through sulfuric acid solution in subsequent acid treatment, solving the problem that alkali solution is directly used for cleaning in the alkali treatment process after acid treatment, and the problem that the residual solid substances cannot be dissolved and cannot be thoroughly cleaned is caused, so as to improve the purification effect, and multiple hydrothermal reactions are also used to improve the consistency of graphite. In actual application, low-concentration sodium hydroxide solution can correspond to low-concentration sulfuric acid solution, and alkaline acid solution neutralization method can be used in later wastewater treatment to minimize sewage treatment costs. In addition, the present invention adds additives during the acid treatment process to regulate the acid treatment environment to improve the utilization efficiency of low-concentration sulfuric acid solution.

[0024] Furthermore, the present invention regulates the sulfuric acid solution by introducing chloride ions and fluoride ions during the acid treatment. After the chloride ions and fluoride ions enter the sulfuric acid solution, they combine with hydrogen ions to form an effect similar to that of adding hydrochloric acid and hydrofluoric acid. However, the use of additives can avoid safety issues caused by the direct use of hydrofluoric acid, and the operability is better during actual application. DETAILED DESCRIPTION

[0025] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.

[0026] In this article, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values ​​within the range (including integers and fractions).

[0027] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”

[0028] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.

[0029] The present invention provides a two-step alkali-acid purification method for natural graphite, comprising the following steps:

[0030] The first step is to mix natural graphite with sodium hydroxide solution, and perform a first hydrothermal reaction to obtain a first intermediate product; the second step is to mix the first intermediate product, sulfuric acid solution and additives, and perform a second hydrothermal reaction to obtain a second intermediate product; the third step is to mix the second intermediate product with sodium hydroxide solution, and perform a third hydrothermal reaction to obtain a third intermediate product; the fourth step is to mix the third intermediate product, sulfuric acid solution and additives, and perform a fourth hydrothermal reaction to obtain purified natural graphite.

[0031] The two-step alkali-acid purification method of natural graphite can increase the purity of natural graphite to more than 99.9%.

[0032] A more specific two-step alkaline acid purification method for natural graphite is as follows:

[0033] S1: Mixing natural graphite with a sodium hydroxide solution having a mass fraction of 2% to 15%, and then performing a first hydrothermal reaction at a temperature of 60°C to 180°C for 1h to 6h to obtain a first intermediate product; wherein the amount ratio of natural graphite to sodium hydroxide solution is 1g: (2.5~10)mL;

[0034] S2: Mix the first intermediate product, a sulfuric acid solution with a mass fraction of 5% to 10%, and an additive, and then perform a second hydrothermal reaction at a temperature of 80°C to 180°C for 1h to 6h to obtain a second intermediate product; wherein the dosage ratio of the first intermediate product to the sulfuric acid solution is 1g: (2.5~10)mL; the additive is composed of fluoride and chloride, and the mass ratio of fluoride to chloride is (1:16) to (3:5); the fluoride is one or both of ammonium fluoride and lithium fluoride, and the chloride is one or both of zinc chloride and lithium chloride, and the dosage of the additive is 5.5% to 9.5% of the mass of the first intermediate product;

[0035] S3: Mix the second intermediate product with a sodium hydroxide solution having a mass fraction of 2% to 15%, and then perform a third hydrothermal reaction at a temperature of 60°C to 180°C for 1h to 6h to obtain a third intermediate product; wherein the amount ratio of the second intermediate product to the sodium hydroxide solution is 1g: (2.5~10)mL;

[0036] S4: The third intermediate product, a sulfuric acid solution with a mass fraction of 5% to 10%, and an additive are mixed, and then a fourth hydrothermal reaction is carried out at a temperature of 80°C to 180°C for 1h to 6h to obtain purified natural graphite; wherein the dosage ratio of the third intermediate product to the sulfuric acid solution is 1g: (2.5~10)mL; the additive is composed of fluoride and chloride, and the mass ratio of fluoride to chloride is (1:16) to (3:5); the fluoride is one or both of ammonium fluoride and lithium fluoride, and the chloride is one or both of zinc chloride and lithium chloride, and the dosage of the additive is 5.5% to 9.5% of the mass of the third intermediate product.

[0037] In the specific implementation process, the reaction conditions of the first hydrothermal reaction and the third hydrothermal reaction are the same; the reaction conditions of the second hydrothermal reaction and the fourth hydrothermal reaction are the same.

[0038] The type of natural graphite can be natural flake graphite or natural spherical graphite, and the above two-step alkali-acid purification method of natural graphite can be applied to the purification of natural flake graphite and natural spherical graphite.

[0039] The present invention adopts a two-step alkali-acid method to purify natural graphite, using a low-concentration alkali solution (a sodium hydroxide solution with a mass fraction of 2% to 15%) and a low-concentration acid solution (a sulfuric acid solution with a mass fraction of 5% to 10%) for purification, and at the same time adding additives to the low-concentration acid solution to introduce chloride ions and fluoride ions to optimize the acid treatment process, thereby improving the safety of the operation and being conducive to industrial application. The purity of the natural graphite purified by the above purification method is above 99.9% and the purity is consistent.

[0040] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0041] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.

[0042] Example 1

[0043] 100 g of natural flake graphite was mixed with 1000 mL of a 2% sodium hydroxide solution, and then subjected to a hydrothermal reaction at 180° C. for 1 hour to obtain a first intermediate product; the first intermediate product was dispersed in 500 mL of a 10% sulfuric acid solution, 3 g of lithium fluoride and 5 g of zinc chloride were added, and then subjected to a hydrothermal reaction at 180° C. for 1 hour to obtain a second intermediate product; the second intermediate product was mixed with 1000 mL of a 2% sodium hydroxide solution, and then subjected to a hydrothermal reaction at 180° C. for 1 hour to obtain a third intermediate product; the third intermediate product was dispersed in 500 mL of a 10% sulfuric acid solution, 3 g of lithium fluoride and 5 g of zinc chloride were added, and then subjected to a hydrothermal reaction at 180° C. for 1 hour to obtain purified natural flake graphite.

[0044] In the calcination experiment test, 2g of purified natural flake graphite was accurately weighed and placed in a porcelain boat with constant weight, and the mass of the purified natural flake graphite and the porcelain boat was recorded; the porcelain boat was placed in a muffle furnace that had been heated to 900℃~1000℃, and after preheating for 1min, it was pushed into the high temperature zone and burned with air flow until there were no black spots; the porcelain boat was taken out and placed in a dryer after cooling slightly, cooled to room temperature, and weighed. By comparing the mass change of the substance in the porcelain boat before and after burning, the mass percentage of ash was calculated, and then the purity of the purified natural flake graphite was obtained.

[0045] After the above calcination experiment test, the purity of the purified natural flake graphite obtained in this embodiment is 99.94%.

[0046] Example 2

[0047] 100 g of natural flake graphite was mixed with 500 mL of a 15% sodium hydroxide solution, and then subjected to a hydrothermal reaction at 60° C. for 6 hours to obtain a first intermediate product; the first intermediate product was dispersed in 1000 mL of a 5% sulfuric acid solution, 1 g of ammonium fluoride and 5 g of zinc chloride were added, and then subjected to a hydrothermal reaction at 80° C. for 6 hours to obtain a second intermediate product; the second intermediate product was mixed with 500 mL of a 15% sodium hydroxide solution, and then subjected to a hydrothermal reaction at 60° C. for 6 hours to obtain a third intermediate product; the third intermediate product was dispersed in 1000 mL of a 5% sulfuric acid solution, 1 g of ammonium fluoride and 5 g of zinc chloride were added, and then subjected to a hydrothermal reaction at 80° C. for 6 hours to obtain purified natural flake graphite.

[0048] In the calcination experiment test, 2g of purified natural flake graphite was accurately weighed and placed in a porcelain boat with constant weight, and the mass of the purified natural flake graphite and the porcelain boat was recorded; the porcelain boat was placed in a muffle furnace that had been heated to 900℃~1000℃, and after preheating for 1min, it was pushed into the high temperature zone and burned with air flow until there were no black spots; the porcelain boat was taken out and placed in a dryer after cooling slightly, cooled to room temperature, and weighed. By comparing the mass change of the substance in the porcelain boat before and after burning, the mass percentage of ash was calculated, and then the purity of the purified natural flake graphite was obtained.

[0049] After the above calcination experiment test, the purity of the purified natural flake graphite obtained in this embodiment is 99.94%.

[0050] Example 3

[0051] 100 g of natural spherical graphite was mixed with 250 mL of a 10% sodium hydroxide solution, and then subjected to a hydrothermal reaction at 90° C. for 3 h to obtain a first intermediate product; the first intermediate product was dispersed in 250 mL of a 6% sulfuric acid solution, 0.5 g of ammonium fluoride and 5 g of lithium chloride were added, and then subjected to a hydrothermal reaction at 150° C. for 3 h to obtain a second intermediate product; the second intermediate product was mixed with 250 mL of a 10% sodium hydroxide solution, and then subjected to a hydrothermal reaction at 90° C. for 3 h to obtain a third intermediate product; the third intermediate product was dispersed in 250 mL of a 6% sulfuric acid solution, 0.5 g of ammonium fluoride and 5 g of lithium chloride were added, and then subjected to a hydrothermal reaction at 150° C. for 3 h to obtain purified natural spherical graphite.

[0052] In the calcination experiment test, 2g of purified natural spherical graphite was accurately weighed and placed in a porcelain boat with constant weight, and the mass of the purified natural spherical graphite and the porcelain boat was recorded; the porcelain boat was placed in a muffle furnace that had been heated to 900℃~1000℃, and after preheating for 1min, it was pushed into the high temperature zone and burned with air flow until there were no black spots; the porcelain boat was taken out and placed in a dryer after cooling slightly, cooled to room temperature, and weighed. By comparing the mass change of the substance in the porcelain boat before and after burning, the mass percentage of ash was calculated, and then the purity of the purified natural spherical graphite was obtained.

[0053] After the above calcination test, the purity of the purified natural spherical graphite obtained in this embodiment is 99.95%.

[0054] Example 4

[0055] 100 g of natural spherical graphite was mixed with 400 mL of a sodium hydroxide solution with a mass fraction of 10%, and then a hydrothermal reaction was carried out at 140° C. for 2 h to obtain a first intermediate product; the first intermediate product was dispersed in 400 mL of a sulfuric acid solution with a mass fraction of 10%, 0.5 g of ammonium fluoride, 5 g of lithium chloride and 3 g of zinc chloride were added, and a hydrothermal reaction was carried out at 140° C. for 2 h to obtain a second intermediate product; the second intermediate product was mixed with 400 mL of a sodium hydroxide solution with a mass fraction of 10%, and then a hydrothermal reaction was carried out at 140° C. for 2 h to obtain a third intermediate product; the third intermediate product was dispersed in 400 mL of a sulfuric acid solution with a mass fraction of 10%, 0.5 g of ammonium fluoride, 5 g of lithium chloride and 3 g of zinc chloride were added, and a hydrothermal reaction was carried out at 140° C. for 2 h to obtain purified natural spherical graphite.

[0056] In the calcination experiment test, 2g of purified natural spherical graphite was accurately weighed and placed in a porcelain boat with constant weight, and the mass of the purified natural spherical graphite and the porcelain boat was recorded; the porcelain boat was placed in a muffle furnace that had been heated to 900℃~1000℃, and after preheating for 1min, it was pushed into the high temperature zone and burned with air flow until there were no black spots; the porcelain boat was taken out and placed in a dryer after cooling slightly, cooled to room temperature, and weighed. By comparing the mass change of the substance in the porcelain boat before and after burning, the mass percentage of ash was calculated, and then the purity of the purified natural spherical graphite was obtained.

[0057] After the above calcination test, the purity of the purified natural spherical graphite obtained in this embodiment is 99.94%.

[0058] Example 5

[0059] 100 g of natural spherical graphite was mixed with 600 mL of a sodium hydroxide solution with a mass fraction of 10%, and then a hydrothermal reaction was carried out at 120° C. for 4 hours to obtain a first intermediate product; the first intermediate product was dispersed in 600 mL of a sulfuric acid solution with a mass fraction of 8%, 0.5 g of ammonium fluoride, 5 g of lithium chloride, 2 g of lithium fluoride and 2 g of zinc chloride were added, and a hydrothermal reaction was carried out at 120° C. for 4 hours to obtain a second intermediate product; the second intermediate product was mixed with 600 mL of a sodium hydroxide solution with a mass fraction of 10%, and then a hydrothermal reaction was carried out at 120° C. for 4 hours to obtain a third intermediate product; the third intermediate product was dispersed in 600 mL of a sulfuric acid solution with a mass fraction of 8%, 0.5 g of ammonium fluoride, 5 g of lithium chloride, 2 g of lithium fluoride and 2 g of zinc chloride were added, and a hydrothermal reaction was carried out at 120° C. for 4 hours to obtain purified natural spherical graphite.

[0060] In the calcination experiment test, 2g of purified natural spherical graphite was accurately weighed and placed in a porcelain boat with constant weight, and the mass of the purified natural spherical graphite and the porcelain boat was recorded; the porcelain boat was placed in a muffle furnace that had been heated to 900℃~1000℃, and after preheating for 1min, it was pushed into the high temperature zone and burned with air flow until there were no black spots; the porcelain boat was taken out and placed in a dryer after cooling slightly, cooled to room temperature, and weighed. By comparing the mass change of the substance in the porcelain boat before and after burning, the mass percentage of ash was calculated, and then the purity of the purified natural spherical graphite was obtained.

[0061] After the above calcination test, the purity of the purified natural spherical graphite obtained in this embodiment is 99.96%.

[0062] Comparative Example 1

[0063] 100 g of natural flake graphite was mixed with 1000 mL of a sodium hydroxide solution with a mass fraction of 40%, and then subjected to a hydrothermal reaction at 180° C. for 1 hour to obtain a first intermediate product; the first intermediate product was dispersed in 500 mL of a sulfuric acid solution with a mass fraction of 50%, 3 g of lithium fluoride and 5 g of zinc chloride were added, and then subjected to a hydrothermal reaction at 180° C. for 1 hour to obtain a second intermediate product; the second intermediate product was mixed with 1000 mL of a sodium hydroxide solution with a mass fraction of 40%, and then subjected to a hydrothermal reaction at 180° C. for 1 hour to obtain a third intermediate product; the third intermediate product was dispersed in 500 mL of a sulfuric acid solution with a mass fraction of 50%, 3 g of lithium fluoride and 5 g of zinc chloride were added, and then subjected to a hydrothermal reaction at 180° C. for 1 hour to obtain purified natural flake graphite.

[0064] In the calcination experiment test, 2g of purified natural flake graphite was accurately weighed and placed in a porcelain boat with constant weight, and the mass of the purified natural flake graphite and the porcelain boat was recorded; the porcelain boat was placed in a muffle furnace that had been heated to 900℃~1000℃, and after preheating for 1min, it was pushed into the high temperature zone and burned with air flow until there were no black spots; the porcelain boat was taken out and placed in a dryer after cooling slightly, cooled to room temperature, and weighed. By comparing the mass change of the substance in the porcelain boat before and after burning, the mass percentage of ash was calculated, and then the purity of the purified natural flake graphite was obtained.

[0065] After the above calcination test, the purity of the purified natural flake graphite obtained in this comparative example is 99.92%.

[0066] By comparing Comparative Example 1 with Example 1, it can be found that the present invention can effectively improve the purity of graphite under low-concentration reaction conditions by optimizing the composition and parameters of the alkaline acid solution.

[0067] When high-concentration sodium hydroxide solution and high-concentration sulfuric acid solution are used for purification, under the same treatment process, the purity of the natural flake graphite in Comparative Example 1 is 99.92%, which is lower than the purity of the natural flake graphite in Example 1. The reason is that the ratio of high-concentration sodium hydroxide solution and high-concentration sulfuric acid solution is not appropriate. In comparison, the low-concentration sodium hydroxide solution and sulfuric acid solution used in the present invention are conducive to improving the purification of natural graphite.

[0068] Comparative Example 2

[0069] 100 g of natural flake graphite was mixed with 1000 mL of 5% sulfuric acid solution, 1 g of ammonium fluoride and 5 g of zinc chloride were added, and a hydrothermal reaction was carried out at 80°C for 6 hours to obtain a first intermediate product; the first intermediate product was mixed with 500 mL of 15% sodium hydroxide solution, and a hydrothermal reaction was carried out at 60°C for 6 hours to obtain a second intermediate product; the second intermediate product was dispersed in 1000 mL of 5% sulfuric acid solution, 1 g of ammonium fluoride and 5 g of zinc chloride were added, and a hydrothermal reaction was carried out at 80°C for 6 hours to obtain a third intermediate product; the third intermediate product was mixed with 500 mL of 15% sodium hydroxide solution, and a hydrothermal reaction was carried out at 60°C for 6 hours to obtain purified natural flake graphite.

[0070] In the calcination experiment test, 2g of purified natural flake graphite was accurately weighed and placed in a porcelain boat with constant weight, and the mass of the purified natural flake graphite and the porcelain boat was recorded; the porcelain boat was placed in a muffle furnace that had been heated to 900℃~1000℃, and after preheating for 1min, it was pushed into the high temperature zone and burned with air flow until there were no black spots; the porcelain boat was taken out and placed in a dryer after cooling slightly, cooled to room temperature, and weighed. By comparing the mass change of the substance in the porcelain boat before and after burning, the mass percentage of ash was calculated, and then the purity of the purified natural flake graphite was obtained.

[0071] After the above calcination test, the purity of the purified natural flake graphite obtained in this comparative example is 99.91%.

[0072] By comparing Comparative Example 2 with Example 2, it can be found that the present invention can improve the purification effect by adjusting the order of alkali and acid treatment.

[0073] As described in the background technology, the existing alkali-acid method for purifying graphite has a process of first acid treatment and then alkali treatment. In theory, alkali treatment can convert silicon and aluminum that are difficult to remove into aluminum silicate and sodium silicate, but the above aluminum silicate and sodium silicate substances are difficult to clean. If the acid-first and then alkali process is used for purification, some solid substances may remain. By comparing Comparative Example 2 with Example 2, it can be seen that the purification effect of first acid treatment and then alkali treatment is lower than the purification effect of first alkali treatment and then acid treatment, which proves the importance of the two-step purification process sequence of first alkali treatment and then acid treatment in the present invention.

[0074] Comparative Example 3

[0075] 100 g of natural spherical graphite was mixed with 250 mL of a 10% sodium hydroxide solution, and then subjected to a hydrothermal reaction at 90° C. for 3 hours to obtain a first intermediate product; the first intermediate product was dispersed in 250 mL of a 6% sulfuric acid solution, and then subjected to a hydrothermal reaction at 150° C. for 3 hours to obtain a second intermediate product; the second intermediate product was mixed with 250 mL of a 10% sodium hydroxide solution, and then subjected to a hydrothermal reaction at 90° C. for 3 hours to obtain a third intermediate product; the third intermediate product was dispersed in 250 mL of a 6% sulfuric acid solution, and then subjected to a hydrothermal reaction at 150° C. for 3 hours to obtain purified natural spherical graphite.

[0076] In the calcination experiment test, 2g of purified natural spherical graphite was accurately weighed and placed in a porcelain boat with constant weight, and the mass of the purified natural spherical graphite and the porcelain boat was recorded; the porcelain boat was placed in a muffle furnace that had been heated to 900℃~1000℃, and after preheating for 1min, it was pushed into the high temperature zone and burned with air flow until there were no black spots; the porcelain boat was taken out and placed in a dryer after cooling slightly, cooled to room temperature, and weighed. By comparing the mass change of the substance in the porcelain boat before and after burning, the mass percentage of ash was calculated, and then the purity of the purified natural spherical graphite was obtained.

[0077] After the above calcination test, the purity of the purified natural spherical graphite obtained in this comparative example is 99.52%.

[0078] By comparing Comparative Example 3 with Example 3, it can be found that the present invention can obtain graphite with higher purity by adding additives during the acid treatment process to control the acidic environment with the additives.

[0079] Comparative Example 3 does not introduce additives during the acid treatment process. Under the same conditions of other treatment parameters, its purification result is lower than the purification result of Example 3, which proves the importance of additives.

[0080] Comparative Example 4

[0081] 100 g of natural spherical graphite was mixed with 400 mL of a 10% sodium hydroxide solution, and then a hydrothermal reaction was carried out at 140° C. for 2 hours to obtain a first intermediate product; the obtained first intermediate product was dispersed in 400 mL of a 10% sulfuric acid solution, 0.5 g of ammonium fluoride, 5 g of lithium chloride and 3 g of zinc chloride were added, and a hydrothermal reaction was carried out at 140° C. for 2 hours to obtain purified natural spherical graphite.

[0082] In the calcination experiment test, 2g of purified natural spherical graphite was accurately weighed and placed in a porcelain boat with constant weight, and the mass of the purified natural spherical graphite and the porcelain boat was recorded; the porcelain boat was placed in a muffle furnace that had been heated to 900℃~1000℃, and after preheating for 1min, it was pushed into the high temperature zone and burned with air flow until there were no black spots; the porcelain boat was taken out and placed in a dryer after cooling slightly, cooled to room temperature, and weighed. By comparing the mass change of the substance in the porcelain boat before and after burning, the mass percentage of ash was calculated, and then the purity of the purified natural spherical graphite was obtained.

[0083] After the above calcination test, the purity of the purified natural spherical graphite obtained in this comparative example is 98.92%.

[0084] By comparing Comparative Example 4 with Example 4, it can be found that the present invention can effectively improve the purity of graphite by combining low-concentration alkali-acid treatment with a two-step alkali-acid method.

[0085] As shown in Comparative Example 4, only one alkali-acid treatment process is used, and the purity of the obtained natural spherical graphite is only 98.92%, which is far below the expected target. The comparison of the purification results of Comparative Example 4 and Example 4 confirms the necessity of combining low-concentration sodium hydroxide solution and sulfuric acid solution with the two-step alkali-acid method.

[0086] In summary, through the comparison of comparative examples and embodiments and analysis of the results, the present invention can improve the purity of natural flake graphite and natural spherical graphite originally having a purity of 90% to 96% to more than 99.9% by optimizing the concentration and formula of the alkaline acid solution, adding additives during the acid treatment process to regulate the acidic environment, and adopting a two-step purification method of first alkaline treatment and then acid treatment.

[0087] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A two-step alkali-acid purification method for natural graphite, characterized in that: The following steps are involved: S1: mixing natural graphite with a sodium hydroxide solution, and then performing a first hydrothermal reaction to obtain a first intermediate product; S2: mixing the first intermediate product, the sulfuric acid solution and the additive, and then performing a second hydrothermal reaction to obtain a second intermediate product; S3: mixing the second intermediate product with a sodium hydroxide solution, and then performing a third hydrothermal reaction to obtain a third intermediate product; S4: mixing the third intermediate product, the sulfuric acid solution and the additive, and then performing a fourth hydrothermal reaction to obtain purified natural graphite; The mass fraction of the sodium hydroxide solution in S1 and S3 is 2% to 15%, and the mass fraction of the sulfuric acid solution in S2 and S4 is 5% to 10%; The additives in S2 and S4 are composed of fluoride and chloride; the mass ratio of the fluoride to the chloride is (1:16) to (3:5); the fluoride is one or both of ammonium fluoride and lithium fluoride, and the chloride is one or both of zinc chloride and lithium chloride.

2. The two-step alkali-acid purification method of natural graphite according to claim 1, characterized in that: In S1, the usage ratio of the natural graphite to the sodium hydroxide solution is 1 g: (2.5-10) mL.

3. The two-step alkali-acid purification method of natural graphite according to claim 1, characterized in that, In S2, the dosage ratio of the first intermediate product to the sulfuric acid solution is 1 g: (2.5-10) mL.

4. The two-step alkali-acid purification method of natural graphite according to claim 1, characterized in that: In S3, the dosage ratio of the second intermediate product to the sodium hydroxide solution is 1 g: (2.5-10) mL.

5. The two-step alkali-acid purification method of natural graphite according to claim 1, characterized in that, In S4, the usage ratio of the third intermediate product to the sulfuric acid solution is 1 g: (2.5-10) mL.

6. The two-step alkali-acid purification method of natural graphite according to claim 1, characterized in that: In S2, the amount of the additive is 5.5% to 9.5% of the mass of the first intermediate product; in S4, the amount of the additive is 5.5% to 9.5% of the mass of the third intermediate product.

7. The two-step alkali-acid purification method of natural graphite according to claim 1, characterized in that: The reaction conditions of the first hydrothermal reaction and the third hydrothermal reaction are the same; the reaction conditions of the first hydrothermal reaction and the third hydrothermal reaction are as follows: the reaction temperature is 60° C. to 180° C., and the reaction time is 1 h to 6 h.

8. The two-step alkali-acid purification method of natural graphite according to claim 1, characterized in that: The reaction conditions of the second hydrothermal reaction and the fourth hydrothermal reaction are the same; the reaction conditions of the second hydrothermal reaction and the fourth hydrothermal reaction are as follows: the reaction temperature is 80° C. to 180° C., and the reaction time is 1 h to 6 h.

9. The two-step alkali-acid purification method of natural graphite according to claim 1, characterized in that: The natural graphite is natural flake graphite or natural spherical graphite.