A method for preparing a rubber composition for a tire inner liner

By using modified white carbon black and composite filler in the tire airtight rubber composition, the problems of unsatisfactory mechanical effects and uneven dispersion of anti-aging agents in the prior art are solved, and the excellent mechanical properties and airtightness of the rubber composition are achieved It extends the anti-aging effect and improves the aging resistance and gas barrier properties of the material.

CN118580613BActive Publication Date: 2024-11-22NANTONG SUNCHI RUBBER PROD CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410881754.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-11-22
Estimated Expiration
2044-07-03

AI Technical Summary

Technical Problem

The existing rubber composition for airtight layers of tires has problems such as unsatisfactory mechanical effects, uneven dispersion of anti-aging agents, poor compatibility of inorganic fillers and rubber compositions, resulting in unstable mechanical properties and deterioration of airtightness.

Method used

By adding modified white carbon black and composite filler, composite filler is prepared by using acid chloride white carbon black and para-phenylenediamine, modified graphene oxide and aniline, modified layered vermiculite sheets and other materials, combined with in-situ polymerization method. Improve the mechanical properties and airtightness of the rubber composition.

Benefits of technology

The mechanical properties and airtightness of the rubber composition are significantly improved, the anti-aging effect is extended, the migration and aggregation of the anti-aging agent is avoided, and the aging resistance and gas barrier properties of the material are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to the field of rubber tires and discloses a method for preparing a rubber composition for a tire airtight layer. The rubber composition comprises the following raw materials in parts by weight: 50-90 parts of brominated butyl rubber, 10-40 parts of natural rubber, 40-60 parts of modified white carbon black, 15-25 parts of a composite filler, 3-8 parts of a tackifying resin, 1-3 parts of stearic acid, 2-5 parts of zinc oxide, 0.5-2 parts of sulfur and 0.5-1.5 parts of an accelerator; the modified white carbon black is acyl chloride white carbon black grafted with a p-phenylenediamine antioxidant; the composite filler is a composite filler prepared by an in-situ polymerization method by mixing modified graphene oxide and modified layered vermiculite flakes and taking aniline as a monomer. The invention provides the rubber composition with excellent mechanical properties, air tightness and aging resistance by adding the modified white carbon black and the composite filler.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of rubber tires, and in particular relates to a method for preparing a rubber composition for a tire airtight layer. Background Art

[0002] Tires are one of the important components of automobiles. Their main function is to support the entire weight of the vehicle, bear the load of the vehicle, transmit traction and braking torque, and ensure the adhesion between the wheel and the road. With the improvement of people's safety and environmental awareness, higher requirements are placed on the performance of tires. The airtight layer is usually located on the inside of the tire. Its main function is to prevent gas leakage in the tire and ensure the stability of the internal air pressure of the tire. The airtightness of the tire is related to the rolling resistance performance, wear performance, handling performance and comfort.

[0003] Currently, the rubber compositions for tire airtight layers mainly use natural rubber, chlorinated butyl rubber and brominated butyl rubber. Due to the presence of a large number of side methyl groups and halogen atoms on the molecular chain of halogenated butyl rubber, the molecular chain has poor activity and therefore has better airtightness. Natural rubber has higher elasticity and excellent mechanical properties, and has a higher Mooney viscosity than other synthetic rubbers, making it easy to process. However, natural rubber contains a large number of unsaturated double bonds in the molecular chain, so it is very easy to age. The existing technology usually adopts the method of adding small molecule antioxidants in the rubber mixing stage to delay rubber aging. However, this method has the disadvantages that the antioxidant is unevenly dispersed and easy to migrate and precipitate. In addition, due to the high price of raw rubber and the problem of unsatisfactory mechanical effect of the rubber composition for the tire airtight layer, in order to reduce material costs and improve mechanical properties, it is necessary to add low-cost inorganic fillers to reduce the rubber content. However, the reduction in the rubber content will have a certain impact on the airtightness of the rubber composition, and the compatibility of inorganic fillers with other raw materials of the rubber composition for the tire airtight layer is not ideal, and there are problems of migration, precipitation and agglomeration, resulting in unstable mechanical properties of the rubber composition for the tire airtight layer. Long-term use will further lead to deterioration of airtightness. Summary of the invention

[0004] In order to solve the deficiencies mentioned in the above background technology, the purpose of the present invention is to provide a method for preparing a rubber composition for a tire airtight layer, by adding modified silica and composite fillers, to give the rubber composition excellent mechanical properties, air tightness and aging resistance.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A rubber composition for a tire airtight layer, comprising the following raw materials in parts by weight: 50-90 parts of brominated butyl rubber, 10-40 parts of natural rubber, 40-60 parts of modified white carbon black, 15-25 parts of composite filler, 3-8 parts of tackifying resin, 1-3 parts of stearic acid, 2-5 parts of zinc oxide, 0.5-2 parts of sulfur, and 0.5-1.5 parts of accelerator;

[0007] The modified silica is acyl chloride silica grafted with p-phenylenediamine antioxidant;

[0008] The composite filler is a composite filler prepared by in-situ polymerization by mixing modified graphene oxide and modified layered vermiculite flakes and using aniline as a monomer, wherein the modified graphene oxide is diethylenetriamine-modified graphene oxide, and the modified layered vermiculite flakes are modified layered vermiculite flakes by using γ-aminopropyltriethoxysilane and succinic anhydride to modify hydroxyl groups and carboxyl groups.

[0009] Preferably, the accelerator is a mixture of one or more of accelerator DM, accelerator TMTD, accelerator DTDM, accelerator MBTS and accelerator NS.

[0010] Preferably, the method for preparing the composite filler comprises the following steps:

[0011] A. Take graphene oxide in N, N-dimethylformamide, disperse it evenly with ultrasonic, add diethylenetriamine and mix, place it at 55-70°C and stir to react for 10-14h, filter and dry after the reaction is completed, and prepare modified graphene oxide;

[0012] B. Grind dried expanded vermiculite in a planetary ball mill to obtain layered vermiculite flakes, take γ-aminopropyltriethoxysilane and succinic anhydride in N,N-dimethylformamide, stir at 70-95°C for 2-5 hours to form a mixed solution, disperse the layered vermiculite flakes in N,N-dimethylformamide, add deionized water after ultrasonic treatment, and then add it to the mixed solution and continue stirring for 4-6 hours. After the reaction is completed, centrifuge, wash and dry to prepare modified layered vermiculite flakes;

[0013] C. Ultrasonic dispersion of modified graphene oxide in deionized water to obtain dispersion 1, ultrasonic dispersion of modified layered vermiculite flakes in deionized water to obtain dispersion 2, uniformly mix dispersion 1 and dispersion 2, add concentrated hydrochloric acid, ultrasonically treat for 40-60 min, adjust the pH of the mixed dispersion to 1.0-1.5, then add aniline, stir at 0-5°C for 1-2 h, then slowly dropwise add ammonium persulfate solution, stir at 0-5°C for 5-8 h after the dropwise addition is completed, filter and dry after the reaction is completed to prepare a composite filler.

[0014] Preferably, in step A, the mass ratio of graphene oxide to diethylenetriamine is 1:18-25.

[0015] Preferably, in step B, the mass ratio of γ-aminopropyltriethoxysilane, succinic anhydride and layered vermiculite flakes is 2-2.5:0.5-1:1-3.

[0016] Preferably, in step B, the ball mill speed is set to 450-700 r / min, and the ball milling time is 15-30 min.

[0017] Preferably, in step C, the mass ratio of the modified graphene oxide, the modified layered vermiculite flakes and the aniline is 1-3:2-5:1.

[0018] Preferably, the preparation method of the modified silica comprises the following steps:

[0019] (1) Ultrasonic dispersion of white carbon black in N,N-dimethylformamide to obtain a dispersion, γ-aminopropyltriethoxysilane and succinic anhydride are stirred in N,N-dimethylformamide for 2-5 hours, and then the dispersion is added, and the mixture is stirred at 40-65°C for 6-8 hours. After the reaction is completed, the mixture is centrifuged, washed, and dried to obtain carboxylated white carbon black;

[0020] (2) Carboxylated silica is dispersed in N,N-dimethylformamide by ultrasonication, dichlorothionyl is added and the mixture is refluxed at 75-80°C for 18-24 hours, and then p-phenylenediamine is added and the mixture is refluxed at 110-125°C in a nitrogen atmosphere for 36-48 hours. After the reaction is completed, the mixture is filtered, washed and dried to prepare modified silica.

[0021] Preferably, the addition ratio of the white carbon black, γ-aminopropyltriethoxysilane, succinic anhydride, thionyl chloride and p-phenylenediamine is 0.2-0.5 g: 10-13 g: 5-7 g: 10-50 mL: 1-2 g.

[0022] A method for preparing the rubber composition for a tire inner liner as described above comprises the following steps:

[0023] S1, a first stage mixing rubber: weigh each raw material by weight, set the temperature of the internal mixer to 120-140°C, the speed to 50-70rpm, add bromobutyl rubber and natural rubber to the internal mixer and mix for 30-60s, lift the top plug, add modified white carbon black, composite filler, stearic acid and tackifying resin, then drop the top plug and mix for 40-80s, then lift the top plug to clean it, press the top plug after cleaning and continue mixing for 30-40s, and control the temperature at 130-140°C to discharge the glue;

[0024] S2, two-stage rubber mixing: add the first-stage rubber mixing into the internal mixer, control the temperature to 80-100°C, the speed to 35-55rpm, lift the top plug after mixing for 30-40s, add sulfur, accelerator and zinc oxide, drop the top plug and mix for 30-60s, then lift the top plug to clean it, press the top plug after cleaning and continue mixing for 30-40s to obtain the final rubber mixing;

[0025] S3, vulcanization: adding the final rubber mixture into a vulcanization mold, controlling the temperature of the vulcanizer to 165-180° C., and vulcanizing for 10-20 min to prepare a rubber composition for a tire airtight layer.

[0026] Beneficial effects of the present invention:

[0027] The invention uses diethylenetriamine to modify graphene oxide, so that the amino group at one end of the diethylenetriamine reacts with the carboxyl group on the surface of the graphene oxide, so that the diethylenetriamine is connected to the graphene oxide, and at the same time, the amino group at the other end of the diethylenetriamine reacts with the phenyl end of the polyaniline molecular chain as an initiator, so that the polyaniline is bonded to the surface of the modified graphene oxide through the NH-C bond, and at the same time, the invention uses a ball milling method to mechanically peel expanded vermiculite to prepare layered vermiculite sheets, and uses γ-aminopropyltriethoxysilane and succinic anhydride to modify the layered vermiculite sheets, so that the surface of the layered vermiculite sheets contains hydroxyl groups and carboxyl groups, so that the modified layered vermiculite sheets and the polyaniline form hydrogen bonds. The invention mixes the modified graphene oxide and the modified layered vermiculite sheets and uses aniline as a monomer, and adopts an in-situ polymerization method to prepare a composite filler, which gives the rubber composition excellent mechanical properties and air tightness. The polyaniline is evenly distributed on the surface of modified graphene oxide and modified layered vermiculite flakes, which increases the compatibility of the composite filler with the rubber matrix and is beneficial to the dispersion of modified graphene oxide and modified layered vermiculite flakes, so that the mechanical properties can be effectively exerted. In addition, when the gas diffuses in the rubber matrix, due to the obstruction of the two-dimensional filler graphene oxide and layered vermiculite flakes, the gas permeation path becomes more tortuous. At the same time, the interaction between the high specific surface area flakes and the polymer molecular chains is stronger, and the free volume between the filler and the molecular chain is smaller, thereby improving the gas barrier performance of the material.

[0028] The invention utilizes gamma-aminopropyltriethoxysilane and succinic anhydride to perform carboxyl modification on white carbon black, then reacts with thionyl chloride to introduce relatively active acyl chloride groups on the surface of the white carbon black, and then reacts with p-phenylenediamine to connect the aniline groups to the surface of the white carbon black through amide bonds, thereby preparing modified white carbon black with anti-aging function. The anti-aging agent p-phenylenediamine is firmly combined with the white carbon black through chemical bonds, and is not easy to decompose and migrate, thereby solving the problem that conventional anti-aging agents are easy to volatilize and migrate from materials, prolonging the anti-aging effect, and at the same time promoting the white carbon black to be relatively evenly dispersed in a rubber matrix, thereby avoiding the performance defects caused by the agglomeration of the white carbon black to a certain extent. DETAILED DESCRIPTION

[0029] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] In the embodiments and comparative examples of the present invention, the brominated butyl rubber is produced by Zhejiang Xinhui New Materials Co., Ltd. with a brand name of 2302, a bromine mass fraction of 1.8-2.2%, and a Mooney viscosity [ML (1+8) 125°C] of 28-36; the expanded vermiculite is produced by Sigma-Aldrich with an average particle size of 2-3 mm; the natural rubber is produced by Zhejiang Sanlishi Rubber Co., Ltd. with a brand name of SCR5; and the tackifying resin is produced by Qingdao Sailun Tire Co., Ltd.

[0031] Embodiment 1 A method for preparing a composite filler comprises the following steps:

[0032] A. Take 2 g of graphene oxide in 50 mL of N,N-dimethylformamide, disperse it evenly with ultrasound, add 50 g of diethylenetriamine and mix, place it at 65 ° C and stir to react for 12 h. After the reaction is completed, filter and dry to prepare modified graphene oxide;

[0033] B. Grind the dried expanded vermiculite in a planetary ball mill to obtain layered vermiculite flakes; add 5 g of γ-aminopropyltriethoxysilane and 2 g of succinic anhydride to 100 mL of N,N-dimethylformamide, stir at 80 ° C for 3 h to form a mixed solution; disperse 5 g of layered vermiculite flakes in 100 mL of N,N-dimethylformamide; add 10 mL of deionized water after ultrasonic treatment; then add the mixture to the mixed solution and continue stirring for 6 h; after the reaction is completed, centrifuge, wash and dry to obtain modified layered vermiculite flakes;

[0034] C. Ultrasonic dispersion of 1 g of modified graphene oxide in 10 mL of deionized water to obtain dispersion 1, ultrasonic dispersion of 4 g of modified layered vermiculite flakes in 40 mL of deionized water to obtain dispersion 2, uniformly mixing dispersion 1 and dispersion 2, adding 10 mL of concentrated hydrochloric acid, ultrasonic treatment for 60 min, adjusting the pH of the mixed dispersion to 1.5, then adding 1 g of aniline, stirring at 5 ° C for 1-2 h, then slowly dropping 10 mL of 24.5% ammonium persulfate solution, stirring and reacting at 5 ° C for 6 h after the dropwise addition is completed, and after the reaction is completed, suction filtration and drying are performed to prepare a composite filler.

[0035] Example 2 A method for preparing modified white carbon black comprises the following steps:

[0036] (1) 0.5 g of white carbon black was uniformly dispersed in 50 mL of N, N-dimethylformamide by ultrasonic dispersion to obtain a dispersion liquid, 11 g of γ-aminopropyltriethoxysilane and 5 g of succinic anhydride were stirred in 50 mL of N, N-dimethylformamide for 3 h, and then the dispersion liquid was added, and the mixture was stirred at 55° C. for 7 h. After the reaction was completed, the mixture was centrifuged, washed, and dried to obtain carboxylated white carbon black;

[0037] (2) Take 0.5 g of carboxylated silica and disperse it in 50 mL of N,N-dimethylformamide with ultrasonic dispersion, add 20 mL of dichlorothionyl and reflux at 80 °C for 24 h, then add 1 g of p-phenylenediamine and reflux at 125 °C in a nitrogen atmosphere for 36 h. After the reaction is completed, filter, wash and dry to prepare modified silica.

[0038] Example 3 A rubber composition for a tire inner liner comprises the following raw materials in parts by weight: 52 parts of brominated butyl rubber, 14 parts of natural rubber, 40 parts of modified silica, 15 parts of composite filler, 3 parts of tackifying resin, 1 part of stearic acid, 2 parts of zinc oxide, 0.5 parts of sulfur, and 0.5 parts of accelerator DM.

[0039] The method for preparing the above-mentioned tire airtight layer rubber composition comprises the following steps:

[0040] S1, a first stage rubber mixing: weigh the above raw materials by weight, set the temperature of the internal mixer to 125 ° C, the speed to 60 rpm, add bromobutyl rubber and natural rubber to the internal mixer and mix for 30 seconds, lift the top plug, add modified white carbon black, composite filler, stearic acid and tackifying resin, then drop the top plug and mix for 80 seconds, then lift the top plug to clean it, press the top plug after cleaning and continue mixing for 40 seconds, and control the temperature at 140 ° C to discharge the glue;

[0041] S2, two-stage rubber mixing: add the first-stage rubber mixing into the internal mixer, control the temperature to 95°C, the speed to 45rpm, lift the top plug after mixing for 30s, add sulfur, accelerator, zinc oxide, and then drop the top plug and mix for 60s, then lift the top plug to clean it, and after cleaning, press the top plug and continue mixing for 40s to obtain the final rubber mixing;

[0042] S3, vulcanization: the final rubber mixture is added into a vulcanization mold, the temperature of the vulcanizer is controlled to be 170° C., and the vulcanization time is 15 min, to prepare a rubber composition for a tire airtight layer.

[0043] Example 4 A rubber composition for a tire inner liner comprises the following raw materials in parts by weight: 74 parts of brominated butyl rubber, 23 parts of natural rubber, 51 parts of modified silica, 20 parts of composite filler, 5 parts of tackifying resin, 2 parts of stearic acid, 4 parts of zinc oxide, 1 part of sulfur, and 1 part of accelerator TMTD.

[0044] The preparation method of the rubber composition for the tire inner liner is the same as that of Example 3.

[0045] Example 5 A rubber composition for a tire inner liner comprises the following raw materials in parts by weight: 87 parts of brominated butyl rubber, 37 parts of natural rubber, 60 parts of modified silica, 25 parts of composite filler, 8 parts of tackifying resin, 3 parts of stearic acid, 5 parts of zinc oxide, 2 parts of sulfur, and 1.5 parts of accelerator MBTS.

[0046] The preparation method of the rubber composition for the tire inner liner is the same as that of Example 3.

[0047] Comparative Example 1 A rubber composition for a tire inner liner comprises the following raw materials in parts by weight: 87 parts of brominated butyl rubber, 37 parts of natural rubber, 60 parts of white carbon black, 25 parts of composite filler, 8 parts of tackifying resin, 3 parts of stearic acid, 5 parts of zinc oxide, 2 parts of sulfur, and 1.5 parts of accelerator MBTS.

[0048] The preparation method of the rubber composition for the tire inner liner is the same as that of Example 3.

[0049] Comparative Example 2 A rubber composition for a tire inner liner comprises the following raw materials in parts by weight: 87 parts of brominated butyl rubber, 37 parts of natural rubber, 60 parts of modified silica, 10 parts of graphene oxide, 15 parts of layered vermiculite flakes, 8 parts of tackifying resin, 3 parts of stearic acid, 5 parts of zinc oxide, 2 parts of sulfur, and 1.5 parts of accelerator MBTS.

[0050] The preparation method of the rubber composition for the tire inner liner is the same as that of Example 3.

[0051] Performance Testing

[0052] (1) The rubber compositions prepared in Examples 3-5 and Comparative Examples 1-2 were subjected to performance tests: tensile stress-strain was tested according to GB / T 528-2009, with a tensile speed of 500 mm / min; tear strength was tested according to GB / T 529-2008, with a tensile speed of 500 mm / min; hardness was tested according to GB / T 39693.7-2022; impact elasticity was tested according to GB / T 1681-2009; fatigue resistance was tested according to GB / T 13934-2006, with a flexion frequency of 300 times / min; airtightness was tested according to GB / T 1038.1-2022, and the data results are shown in Table 1.

[0053] Table 1 Test results of sample performance

[0054]

[0055] It can be seen from the data in Table 1 that the rubber compositions prepared in Examples 3-5 of the present invention have high tensile strength and tear strength, are not easy to break, and have good fatigue resistance and air tightness. In Comparative Example 1, white carbon black was not modified, and the mechanical properties measured were slightly worse than those of Examples 3-5. In Comparative Example 2, graphene oxide and layered vermiculite flakes were simply blended, and the mechanical properties measured were significantly lower than those of Examples 3-5, and the air permeability increased, and the air tightness became worse.

[0056] (2) The rubber compositions prepared in Examples 3-5 and Comparative Examples 1-2 were subjected to hot air aging tests in accordance with GB / T 3512-2014 at an aging temperature of 100° C. The changes in tensile strength and elongation at break were tested. The data obtained are shown in Table 2 below.

[0057] Table 2 Test of heat aging resistance of samples

[0058]

[0059] It can be seen from the data in Table 2 that the rubber compositions prepared in Examples 3-5 of the present invention still have high tensile strength and elongation at break after aging for 24h and 72h, and have excellent aging resistance. Among them, the tensile strength and elongation at break of the rubber composition prepared in Comparative Example 1 after aging are significantly reduced compared with those in Examples 3-5, indicating that modification of silica can improve the aging resistance of the rubber composition.

[0060] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0061] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.

Claims

1. A rubber composition for a tire inner liner, characterized in that: The invention comprises the following raw materials in parts by weight: 50-90 parts of brominated butyl rubber, 10-40 parts of natural rubber, 40-60 parts of modified white carbon black, 15-25 parts of composite filler, 3-8 parts of tackifying resin, 1-3 parts of stearic acid, 2-5 parts of zinc oxide, 0.5-2 parts of sulfur and 0.5-1.5 parts of accelerator; The modified silica is acyl chloride silica grafted with p-phenylenediamine antioxidant; The composite filler is a composite filler prepared by in-situ polymerization by mixing modified graphene oxide and modified layered vermiculite flakes with aniline as a monomer, wherein the modified graphene oxide is diethylenetriamine-modified graphene oxide, and the modified layered vermiculite flakes are modified layered vermiculite flakes modified with hydroxyl and carboxyl groups by using γ-aminopropyltriethoxysilane and succinic anhydride; The mass ratio of the graphene oxide to diethylenetriamine is 1:18-25; the mass ratio of the γ-aminopropyltriethoxysilane, succinic anhydride and layered vermiculite flakes is 2-2.5:0.5-1:1-3; the mass ratio of the modified graphene oxide, modified layered vermiculite flakes and aniline is 1-3:2-5:1; The preparation method of the modified white carbon black comprises the following steps: (1) Ultrasonic dispersion of white carbon black in N,N-dimethylformamide to obtain a dispersion, γ-aminopropyltriethoxysilane and succinic anhydride are stirred in N,N-dimethylformamide for 2-5 hours, and then the dispersion is added, and the mixture is stirred at 40-65°C for 6-8 hours. After the reaction is completed, the mixture is centrifuged, washed, and dried to obtain carboxylated white carbon black; (2) Carboxylated silica is ultrasonically dispersed in N,N-dimethylformamide, dichlorothionyl is added and refluxed at 75-80°C for 18-24 hours, and then p-phenylenediamine is added and refluxed at 110-125°C in a nitrogen atmosphere for 36-48 hours. After the reaction is completed, the modified silica is filtered, washed and dried to prepare the modified silica; In the step (1), the mass ratio of white carbon black, γ-aminopropyltriethoxysilane and succinic anhydride is 0.5:11:5; and in the step (2), the addition ratio of carboxylated white carbon black, dichlorothionyl and p-phenylenediamine is 0.5 g:20 mL:1 g.

2. The rubber composition for a tire inner liner according to claim 1, characterized in that: The accelerator is a mixture of one or more of accelerator DM, accelerator TMTD, accelerator DTDM, accelerator MBTS and accelerator NS.

3. The rubber composition for a tire inner liner according to claim 1, characterized in that: The preparation method of the composite filler comprises the following steps: A. Take graphene oxide in N, N-dimethylformamide, disperse it evenly with ultrasonic, add diethylenetriamine and mix, place it at 55-70°C and stir to react for 10-14h, filter and dry after the reaction is completed, and prepare modified graphene oxide; B. Grind dried expanded vermiculite in a planetary ball mill to obtain layered vermiculite flakes, take γ-aminopropyltriethoxysilane and succinic anhydride in N,N-dimethylformamide, stir at 70-95°C for 2-5 hours to form a mixed solution, disperse the layered vermiculite flakes in N,N-dimethylformamide, add deionized water after ultrasonic treatment, and then add it to the mixed solution and continue stirring for 4-6 hours. After the reaction is completed, centrifuge, wash and dry to prepare modified layered vermiculite flakes; C. Ultrasonic dispersion of modified graphene oxide in deionized water to obtain dispersion 1, ultrasonic dispersion of modified layered vermiculite flakes in deionized water to obtain dispersion 2, uniformly mix dispersion 1 and dispersion 2, add concentrated hydrochloric acid, ultrasonically treat for 40-60 min, adjust the pH of the mixed dispersion to 1.0-1.5, then add aniline, stir at 0-5°C for 1-2 h, then slowly dropwise add ammonium persulfate solution, stir at 0-5°C for 5-8 h after the dropwise addition is completed, filter and dry after the reaction is completed to prepare a composite filler.

4. The rubber composition for a tire inner liner according to claim 3, characterized in that: In step B, the ball mill speed is set to 450-700 r / min, and the ball milling time is 15-30 min.

5. A method for preparing the rubber composition for a tire inner liner according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1, a first stage mixing rubber: weigh each raw material by weight, set the temperature of the internal mixer to 120-140°C, the speed to 50-70rpm, add bromobutyl rubber and natural rubber to the internal mixer and mix for 30-60s, lift the top plug, add modified white carbon black, composite filler, stearic acid and tackifying resin, then drop the top plug and mix for 40-80s, then lift the top plug to clean it, press the top plug after cleaning and continue mixing for 30-40s, and control the temperature at 130-140°C to discharge the glue; S2, two-stage rubber mixing: add the first-stage rubber mixing into the internal mixer, control the temperature to 80-100°C, the speed to 35-55rpm, lift the top plug after mixing for 30-40s, add sulfur, accelerator and zinc oxide, drop the top plug and mix for 30-60s, then lift the top plug to clean it, press the top plug after cleaning and continue mixing for 30-40s to obtain the final rubber mixing; S3, vulcanization: adding the final rubber mixture into a vulcanization mold, controlling the temperature of the vulcanizer to 165-180° C., and vulcanizing for 10-20 min to prepare a rubber composition for a tire airtight layer.

Citation Information

Patent Citations

  • A preparation method for porous graphene and a preparation method for a graphene-based aluminium-air cell

    CN103387229A

  • Expanded vermiculite powder modified anti-corrosion epoxy resin composite material for LED bonding layer and preparation method thereof

    CN106753128A

  • High-gas-preservation easy bonding shaping low-cost tire airtightness layer glue composition

    CN108384130A

  • Tyre inner lining glue with graphene / carbon black composite and preparation method of tyre inner lining glue

    CN109161110A

  • Polyvinyl chloride medicine package sheet with anti-fouling and anti-bacterial functions and preparation method of polyvinyl chloride medicine package sheet

    CN114644771A