A weather-resistant polymer waterproof material for roofing
By using the core-shell structure and branched structure of modified prepolymers and modified fillers in the roof waterproofing material, the problem of poor weather resistance of waterproofing materials in the prior art is solved, and higher waterproofing performance and service life are achieved.
Patent Information
- Application Number
- CN202411035595.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-07-31
AI Technical Summary
At this stage, the weather resistance of roof waterproof materials is poor, and they are prone to aging and lead to water leakage after long-term use.
Using a roof weather-resistant polymer waterproof material, through the blending of component A and component B, component A is a modified prepolymer, component B includes polyether 330N, talc, modified filler, methyl trimethyl The modified prepolymer is made by specific reaction steps to form a core-shell structure and branched structure. Improve mechanical properties and waterproofing.
It significantly improves the weather resistance and waterproof performance of waterproof materials, extends the service life, and slows down the aging reaction by reflecting ultraviolet light and absorbing excited energy from the modified filler.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waterproof material preparation, and in particular to a weather-resistant polymer waterproof material for roofing. Background Art
[0002] Roofing waterproof materials are exposed waterproof materials used on the roofs of buildings. They are mainly divided into roll materials and coatings. Compared with roll materials, coatings are lighter and can be applied to substrates of different shapes. Specifically, they can be divided into acrylic systems, polyurethane systems, etc. The polyurethane system is a waterproof coating obtained by the reaction of excess isocyanate monomers with polyether polyols to generate a polyurethane prepolymer containing residual isocyanate groups, which is then compounded with cross-linking agents, pigments, fillers, solvents, etc. The waterproof coating has good extensibility and substrate adhesion, and is particularly suitable for construction on substrates with complex structures or non-planar surfaces. It is therefore favored by the waterproofing community at home and abroad and is widely used in waterproofing projects such as roofs, basements, kitchens and bathrooms, water tanks, subways, bridges, and parking lots. However, the coating will show obvious aging after long-term use, resulting in a decrease in or even disappearance of the waterproof performance. Summary of the invention
[0003] The purpose of the present invention is to provide a weather-resistant polymer waterproof material for roofing, which solves the problem that the weather-resistant performance of waterproof materials at present is average and aging and water leakage will occur after long-term use.
[0004] The purpose of the present invention can be achieved through the following technical solutions:
[0005] A weather-resistant polymer waterproof material for roofing, comprising component A and component B in a mass ratio of 1:2, wherein component A is a modified prepolymer, and component B comprises the following raw materials in parts by weight: 40-50 parts of polyether 330N, 1-3 parts of dibutyltin dilaurate, 5-10 parts of talc, 10-15 parts of modified filler, 3-5 parts of methyltrimethoxysilane, 3-5 parts of dimethyldimethoxysilane, 3-5 parts of phenyltrimethoxysilane, 1-3 parts of dispersant, 1-3 parts of defoamer and 30-50 parts of xylene;
[0006] The modified prepolymer is prepared by the following steps:
[0007] Step S1: 2,2-dihydroxymethylpropionic acid, KH550, dicyclohexylcarbodiimide and toluene are mixed evenly, and reacted for 3-5 hours at a speed of 200-300 r / min and a temperature of 40-50° C. to obtain a chain extension monomer; methyltrifluoropropylcyclotrisiloxane, octamethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, tetramethylammonium hydroxide and dimethyl sulfoxide are mixed evenly, and nitrogen is introduced for protection. After reacting for 2-4 hours at a speed of 120-150 r / min and a temperature of 90-95° C., the temperature is raised to 140-150° C. and kept warm for 1-1.5 hours to obtain a diamine-terminated polysiloxane;
[0008] Step S2: 2-perfluorooctylethanol, epichlorohydrin, tetrabutylammonium bromide and DMF are mixed evenly, nitrogen is introduced for protection, and the reaction is carried out for 2-3 hours at a speed of 120-150 r / min and a temperature of 110-120° C., and the temperature is lowered to 50-55° C., and a sodium hydroxide solution is added to react for 6-8 hours to obtain a modifier, and the modifier, diamine-terminated polysiloxane and DMF are mixed evenly, and the reaction is carried out for 4-6 hours at a speed of 150-200 r / min, a temperature of 20-25° C. and a pH value of 10-11 to obtain a waterproof monomer;
[0009] Step S3: uniformly mix the modified monomer, waterproof monomer and polyether 220, introduce nitrogen, stir and add diphenylmethane diisocyanate at a speed of 120-150r / min and a temperature of 85-90°C, react for 2-3h, add a chain extension monomer, continue the reaction for 2-3h, and obtain a modified prepolymer.
[0010] Furthermore, the molar ratio of 2,2-dihydroxymethylpropionic acid, KH550 and dicyclohexylcarbodiimide in step S1 is 1:1:1.2, and the molar ratio of methyltrifluoropropylcyclotrisiloxane, octamethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and tetramethylammonium hydroxide is 0.5:1.2:3.75:2.5.
[0011] Furthermore, the 2-perfluorooctylethanol, epichlorohydrin, tetrabutylammonium bromide and sodium hydroxide solution described in step S2 are 20mmol:20mmol:0.1g:10mL, the mass fraction of the sodium hydroxide solution is 60%, and the molar ratio of the modifier to the double-terminal polysiloxane is 4:1.
[0012] Furthermore, the molar ratio of the modified monomer, waterproof monomer, polyether 220, diphenylmethane diisocyanate and chain extension monomer described in step S3 is 1:2:5:12:1.
[0013] Further, the modified monomer is prepared by the following steps:
[0014] Step A1: Mix magnesium chips, iodine, 4-bromoanisole and tetrahydrofuran, introduce nitrogen protection, stir for 2-3 hours at a speed of 120-150 r / min and a temperature of 60-70° C., cool to 0-5° C., add cyanuric chloride, and continue to react for 3-5 hours to obtain intermediate 1; mix intermediate 1, resorcinol, xylene and cyclopentane sulfone, introduce nitrogen protection, stir and add aluminum chloride at a speed of 120-150 r / min and a temperature of 80-90° C., and react for 4-6 hours to obtain intermediate 2;
[0015] Step A2: The intermediate 2, potassium carbonate, sodium chloroacetate and DMF are mixed evenly, reacted at a speed of 200-300 r / min and a temperature of 90-100° C. for 6-8 hours, and the pH value is adjusted to 6-6.5 to obtain the intermediate 3. The intermediate 3, diethanolamine, dicyclohexylcarbodiimide and toluene are mixed evenly, reacted at a speed of 120-150 r / min and a temperature of 110-120° C. for 5-7 hours to obtain the modified monomer.
[0016] Furthermore, the molar ratio of magnesium chips, iodine, 4-bromoanisole and cyanuric chloride described in step A1 is 50mmol:1mg:50mmol:50mmol, and the molar ratio of intermediate 1, resorcinol and aluminum chloride is 1:2:2.5.
[0017] Furthermore, the usage ratio of the intermediate 2, potassium carbonate and sodium chloroacetate in step A2 is 1:2:2, and the molar ratio of the intermediate 3, diethanolamine and dicyclohexylcarbodiimide is 1:2:2.1.
[0018] Further, the modified filler is prepared by the following steps:
[0019] Step B1: dissolving nickel nitrate hexahydrate in DMF, stirring and adding aminoterephthalic acid and 2-methylimidazole at a speed of 150-200 r / min and a temperature of 30-40° C., stirring for 1-2 hours, heating to 180-185° C., reacting for 20-25 hours to obtain a nickel metal organic framework, and uniformly mixing the nickel metal organic framework, KH560 and DMF, reacting for 5-7 hours at a speed of 200-300 r / min, a temperature of 20-25° C., and a pH value of 10-11 to obtain a modified nickel framework;
[0020] Step B2: The modified nickel framework, acetonitrile, isopropanol, KH550 and tetraethylammonium hydroxide are mixed evenly, and deionized water is added under the conditions of a rotation speed of 120-150r / min and a temperature of 50-55°C, and the reaction is carried out for 20-25h to obtain a precursor. The precursor, zinc nitrate hexahydrate and deionized water are mixed evenly, and ammonia water is added under the conditions of a rotation speed of 600-800r / min and a temperature of 30-40°C. After stirring for 20-30min, hydrogen peroxide is added, and the reaction is continued for 3-5h to obtain a modified filler.
[0021] Furthermore, the molar ratio of nickel nitrate hexahydrate, aminoterephthalic acid and 2-methylimidazole in step B1 is 2:1:1, and the molar ratio of the amino group on the nickel metal organic framework and KH560 is 1:1.
[0022] Furthermore, the modified nickel framework, acetonitrile, isopropanol, KH550, tetraethylammonium hydroxide and deionized water in step B2 are used in a ratio of 3 g: 5 mL: 10 mL: 10 mL: 5 mL: 20 mL, and the precursor, zinc nitrate hexahydrate, deionized water, ammonia water and hydrogen peroxide are used in a ratio of 1 g: 3 g: 20 mL: 1.6 mL: 1.5 mL.
[0023] Beneficial effects of the invention: A weather-resistant polymer waterproof material for roofing disclosed in the present application comprises component A and component B, wherein component A is a modified prepolymer, and component B comprises the following raw materials in parts by weight: polyether 330N, dibutyltin dilaurate, talcum powder, modified filler, methyltrimethoxysilane, dimethyldimethoxysilane, phenyltrimethoxysilane, dispersant, defoamer and xylene, wherein the modified prepolymer is subjected to a dehydration reaction with 2,2-dimethylolpropionic acid and KH550 under the action of dicyclohexylcarbodiimide, so that the carboxyl group on the 2,2-dimethylolpropionic acid reacts with the amino group on the KH550 to obtain a chain extension monomer, and methyltrifluoropropylcyclotrisiloxane and Octamethylcyclotetrasiloxane is ring-opened and polymerized with 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane to obtain diamine-terminated polysiloxane, 2-perfluorooctylethanol is reacted with epichlorohydrin so that the hydroxyl group of 2-perfluorooctylethanol reacts with the epoxy group on epichlorohydrin, and then the ring is closed under the action of sodium hydroxide solution to obtain a modifier, the modifier is reacted with diamine-terminated polysiloxane so that the epoxy group on the modifier reacts with the amino group on the diamine-terminated polysiloxane to form a new hydroxyl group to obtain a waterproof monomer, and the waterproof monomer, the modified monomer, polyether 220, diphenylmethane diisocyanate and the chain extension monomer are reacted to obtain a modified prepolymer.
[0024] The modified monomer is reacted with magnesium chips, iodine and 4-bromoanisole to form a Grignard reagent, which reacts with a chlorine atom site on cyanuric chloride to obtain an intermediate 1, and the intermediate 1 is reacted with resorcinol to react with the remaining chlorine atom sites on the intermediate 1 to obtain an intermediate 2, and the intermediate 2 is reacted with sodium chloroacetate to react with the phenolic hydroxyl group on the intermediate 2 and the chlorine atom site of the sodium chloroacetate, and then the acid is adjusted to convert the sodium acetate into acetic acid to obtain an intermediate 3, and the intermediate 3 is reacted with ethylene glycol amine to react with the carboxyl group on the intermediate 3 and the secondary amine on the ethylene glycol amine to obtain the modified monomer.
[0025] The modified filler is prepared by reacting nickel nitrate hexahydrate, aminoterephthalic acid and 2-methylimidazole to obtain a nickel metal organic framework, which is then reacted with KH560 so that the amino groups on the nickel metal organic framework react with the epoxy groups on KH560 to obtain a modified nickel framework, which is then reacted with KH550 to form a cage-type silsesquioxane structure on the surface to obtain a precursor, and zinc peroxide is loaded on the precursor using zinc nitrate hexahydrate as a raw material to obtain a modified filler.
[0026] During the blending process of component A and component B, the amino group on the surface of the modified filler can react with the isocyanate group in the modified prepolymer to form a core-shell structure in which the prepolymer molecule encapsulates the modified filler. At the same time, the core-shell contains a cage-type silsesquioxane structure, which is combined with the branched structure of the modified prepolymer to improve the mechanical properties of the waterproof material. The side chain of the modified prepolymer contains a siloxane structure. During the curing and use of the material, it comes into contact with moisture in the air. The siloxane, methyltrimethoxysilane, dimethyldimethoxysilane and phenyltrimethoxysilane in the side chain of the modified prepolymer can undergo hydrolysis and condensation, and can be combined with the fluorocarbon segment and the polysiloxane segment to greatly improve the waterproof effect. The molecule contains a six-membered chelate ring, which converts energy through the closing and opening process of the six-membered chelate ring to increase the weather resistance of the material. The modified filler can reflect part of the ultraviolet light to contact the matrix, while absorbing the excited state energy in the matrix to slow down the aging reaction. DETAILED DESCRIPTION
[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1
[0028] A weather-resistant polymer waterproof material for roofing, comprising component A and component B in a mass ratio of 1:2, wherein component A is a modified prepolymer, and component B comprises the following raw materials in parts by weight: 40 parts of polyether 330N, 1 part of dibutyltin dilaurate, 5 parts of talcum powder, 10 parts of modified fillers, 3 parts of methyltrimethoxysilane, 3 parts of dimethyldimethoxysilane, 3 parts of phenyltrimethoxysilane, 1 part of dispersant, 1 part of defoamer and 30 parts of xylene;
[0029] The dispersant is F108, and the defoamer is DF831.
[0030] The modified prepolymer is prepared by the following steps:
[0031] Step S1: 2,2-dihydroxymethylpropionic acid, KH550, dicyclohexylcarbodiimide and toluene are mixed evenly, and reacted at a speed of 200 r / min and a temperature of 40° C. for 3 h to obtain a chain extension monomer; methyltrifluoropropylcyclotrisiloxane, octamethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, tetramethylammonium hydroxide and dimethyl sulfoxide are mixed evenly, and nitrogen is introduced for protection, and reacted at a speed of 120 r / min and a temperature of 90° C. for 2 h, and then the temperature is raised to 140° C. and kept for h to obtain a diamine-terminated polysiloxane;
[0032] Step S2: 2-perfluorooctylethanol, epichlorohydrin, tetrabutylammonium bromide and DMF are mixed evenly, nitrogen is introduced for protection, and the mixture is reacted for 2 hours at a speed of 120 r / min and a temperature of 110° C., then the temperature is lowered to 50° C., sodium hydroxide solution is added, and the mixture is reacted for 6 hours to obtain a modifier, and the modifier, diamine-terminated polysiloxane and DMF are mixed evenly, and the mixture is reacted for 4 hours at a speed of 150 r / min, a temperature of 20° C. and a pH value of 10 to obtain a waterproof monomer;
[0033] Step S3: uniformly mix the modified monomer, waterproof monomer and polyether 220, introduce nitrogen, stir and add diphenylmethane diisocyanate at a speed of 120 r / min and a temperature of 85°C, react for 2 hours, add a chain extension monomer, and continue the reaction for 2 hours to obtain a modified prepolymer.
[0034] The molar ratio of 2,2-dihydroxymethylpropionic acid, KH550 and dicyclohexylcarbodiimide in step S1 is 1:1:1.2, and the molar ratio of methyltrifluoropropylcyclotrisiloxane, octamethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and tetramethylammonium hydroxide is 0.5:1.2:3.75:2.5.
[0035] The 2-perfluorooctylethanol, epichlorohydrin, tetrabutylammonium bromide and sodium hydroxide solution described in step S2 are 20mmol:20mmol:0.1g:10mL, the mass fraction of the sodium hydroxide solution is 60%, and the molar ratio of the modifier to the double-terminal polysiloxane is 4:1.
[0036] The molar ratio of the modified monomer, waterproof monomer, polyether 220, diphenylmethane diisocyanate and chain extension monomer described in step S3 is 1:2:5:12:1.
[0037] The modified monomer is prepared by the following steps:
[0038] Step A1: Mix magnesium chips, iodine, 4-bromoanisole and tetrahydrofuran, introduce nitrogen protection, stir for 2 hours at a speed of 120 r / min and a temperature of 60° C., cool to 0° C., add cyanuric chloride, and continue to react for 3 hours to obtain intermediate 1; mix intermediate 1, resorcinol, xylene and cyclopentane sulfone, introduce nitrogen protection, stir and add aluminum chloride at a speed of 120 r / min and a temperature of 80° C., and react for 4 hours to obtain intermediate 2;
[0039] Step A2: The intermediate 2, potassium carbonate, sodium chloroacetate and DMF are mixed evenly, reacted at a speed of 200 r / min and a temperature of 90°C for 6 hours, and then the pH value is adjusted to 6 to obtain the intermediate 3. The intermediate 3, diethanolamine, dicyclohexylcarbodiimide and toluene are mixed evenly, reacted at a speed of 120 r / min and a temperature of 110°C for 5 hours to obtain the modified monomer.
[0040] The molar ratio of magnesium chips, iodine, 4-bromoanisole and cyanuric chloride described in step A1 is 50mmol:1mg:50mmol:50mmol, and the molar ratio of intermediate 1, resorcinol and aluminum chloride is 1:2:2.5.
[0041] The usage ratio of intermediate 2, potassium carbonate and sodium chloroacetate in step A2 is 1:2:2, and the molar ratio of intermediate 3, diethanolamine and dicyclohexylcarbodiimide is 1:2:2.1.
[0042] The modified filler is prepared by the following steps:
[0043] Step B1: dissolving nickel nitrate hexahydrate in DMF, stirring and adding aminoterephthalic acid and 2-methylimidazole at a speed of 150 r / min and a temperature of 30° C., stirring for 1 hour, heating to 180° C., reacting for 20 hours to obtain a nickel metal organic framework, and mixing the nickel metal organic framework, KH560 and DMF uniformly, reacting for 5 hours at a speed of 200 r / min, a temperature of 20° C. and a pH value of 10 to obtain a modified nickel framework;
[0044] Step B2: The modified nickel framework, acetonitrile, isopropanol, KH550 and tetraethylammonium hydroxide are mixed evenly, and deionized water is added under the conditions of a rotation speed of 120 r / min and a temperature of 50°C, and the reaction is carried out for 20 hours to obtain a precursor. The precursor, zinc nitrate hexahydrate and deionized water are mixed evenly, and ammonia water is added under the conditions of a rotation speed of 600 r / min and a temperature of 30°C. After stirring for 20 minutes, hydrogen peroxide is added, and the reaction is continued for 3 hours to obtain a modified filler.
[0045] The molar ratio of nickel nitrate hexahydrate, aminoterephthalic acid and 2-methylimidazole in step B1 is 2:1:1, and the molar ratio of the amino group on the nickel metal organic framework and KH560 is 1:1.
[0046] The modified nickel framework, acetonitrile, isopropanol, KH550, tetraethylammonium hydroxide and deionized water in step B2 are used in a ratio of 3 g: 5 mL: 10 mL: 10 mL: 5 mL: 20 mL, and the precursor, zinc nitrate hexahydrate, deionized water, ammonia water and hydrogen peroxide are used in a ratio of 1 g: 3 g: 20 mL: 1.6 mL: 1.5 mL. Example 2
[0047] A weather-resistant polymer waterproof material for roofing, comprising component A and component B in a mass ratio of 1:2, wherein component A is a modified prepolymer, and component B comprises the following raw materials in parts by weight: 45 parts of polyether 330N, 2 parts of dibutyltin dilaurate, 8 parts of talcum powder, 13 parts of modified filler, 4 parts of methyltrimethoxysilane, 4 parts of dimethyldimethoxysilane, 4 parts of phenyltrimethoxysilane, 2 parts of dispersant, 2 parts of defoamer and 40 parts of xylene;
[0048] The dispersant is 5027 and the defoamer is DF530.
[0049] The modified prepolymer is prepared by the following steps:
[0050] Step S1: 2,2-dihydroxymethylpropionic acid, KH550, dicyclohexylcarbodiimide and toluene are mixed evenly, and reacted at a speed of 200 r / min and a temperature of 45° C. for 4 hours to obtain a chain extension monomer; methyltrifluoropropylcyclotrisiloxane, octamethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, tetramethylammonium hydroxide and dimethyl sulfoxide are mixed evenly, and nitrogen is introduced for protection. After reacting at a speed of 120 r / min and a temperature of 93° C. for 3 hours, the temperature is raised to 145° C. and kept warm for 1.3 hours to obtain a diamine-terminated polysiloxane;
[0051] Step S2: 2-perfluorooctylethanol, epichlorohydrin, tetrabutylammonium bromide and DMF are mixed evenly, nitrogen is introduced for protection, and the reaction is carried out for 2.5 hours at a speed of 120 r / min and a temperature of 115° C., and the temperature is lowered to 53° C., sodium hydroxide solution is added, and the reaction is carried out for 7 hours to obtain a modifier, and the modifier, diamine-terminated polysiloxane and DMF are mixed evenly, and the reaction is carried out for 5 hours at a speed of 150 r / min, a temperature of 23° C. and a pH value of 11 to obtain a waterproof monomer;
[0052] Step S3: uniformly mix the modified monomer, waterproof monomer and polyether 220, introduce nitrogen, stir and add diphenylmethane diisocyanate at a speed of 120 r / min and a temperature of 88°C, react for 2.5 hours, add a chain extension monomer, continue the reaction for 2-3 hours, and obtain a modified prepolymer.
[0053] The molar ratio of 2,2-dihydroxymethylpropionic acid, KH550 and dicyclohexylcarbodiimide in step S1 is 1:1:1.2, and the molar ratio of methyltrifluoropropylcyclotrisiloxane, octamethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and tetramethylammonium hydroxide is 0.5:1.2:3.75:2.5.
[0054] The 2-perfluorooctylethanol, epichlorohydrin, tetrabutylammonium bromide and sodium hydroxide solution described in step S2 are 20mmol:20mmol:0.1g:10mL, the mass fraction of the sodium hydroxide solution is 60%, and the molar ratio of the modifier to the double-terminal polysiloxane is 4:1.
[0055] The molar ratio of the modified monomer, waterproof monomer, polyether 220, diphenylmethane diisocyanate and chain extension monomer described in step S3 is 1:2:5:12:1.
[0056] The modified monomer is prepared by the following steps:
[0057] Step A1: Magnesium chips, iodine, 4-bromoanisole and tetrahydrofuran are mixed uniformly, nitrogen is introduced for protection, and the mixture is stirred for 2.5 hours at a speed of 120 r / min and a temperature of 65° C., then the temperature is lowered to 3° C., cyanuric chloride is added, and the reaction is continued for 4 hours to obtain intermediate 1; intermediate 1, resorcinol, xylene and cyclopentane are mixed uniformly, nitrogen is introduced for protection, aluminum chloride is added at a speed of 120 r / min and a temperature of 85° C., and the mixture is stirred for 5 hours to obtain intermediate 2;
[0058] Step A2: The intermediate 2, potassium carbonate, sodium chloroacetate and DMF are mixed evenly, reacted at a speed of 200 r / min and a temperature of 95°C for 7 hours, and then the pH value is adjusted to 6 to obtain the intermediate 3. The intermediate 3, diethanolamine, dicyclohexylcarbodiimide and toluene are mixed evenly, reacted at a speed of 120 r / min and a temperature of 115°C for 6 hours to obtain the modified monomer.
[0059] The molar ratio of magnesium chips, iodine, 4-bromoanisole and cyanuric chloride described in step A1 is 50mmol:1mg:50mmol:50mmol, and the molar ratio of intermediate 1, resorcinol and aluminum chloride is 1:2:2.5.
[0060] The usage ratio of intermediate 2, potassium carbonate and sodium chloroacetate in step A2 is 1:2:2, and the molar ratio of intermediate 3, diethanolamine and dicyclohexylcarbodiimide is 1:2:2.1.
[0061] The modified filler is prepared by the following steps:
[0062] Step B1: dissolving nickel nitrate hexahydrate in DMF, stirring and adding aminoterephthalic acid and 2-methylimidazole at a speed of 150 r / min and a temperature of 35° C., stirring for 1.5 hours, heating to 180° C., reacting for 23 hours to obtain a nickel metal organic framework, and mixing the nickel metal organic framework, KH560 and DMF uniformly, reacting for 6 hours at a speed of 300 r / min, a temperature of 23° C. and a pH value of 10 to obtain a modified nickel framework;
[0063] Step B2: The modified nickel framework, acetonitrile, isopropanol, KH550 and tetraethylammonium hydroxide are mixed evenly, and deionized water is added under the conditions of a rotation speed of 120 r / min and a temperature of 53°C, and the reaction is carried out for 23 hours to obtain a precursor. The precursor, zinc nitrate hexahydrate and deionized water are mixed evenly, and ammonia water is added under the conditions of a rotation speed of 600 r / min and a temperature of 35°C. After stirring for 25 minutes, hydrogen peroxide is added, and the reaction is continued for 4 hours to obtain a modified filler.
[0064] The molar ratio of nickel nitrate hexahydrate, aminoterephthalic acid and 2-methylimidazole in step B1 is 2:1:1, and the molar ratio of the amino group on the nickel metal organic framework and KH560 is 1:1.
[0065] The modified nickel framework, acetonitrile, isopropanol, KH550, tetraethylammonium hydroxide and deionized water in step B2 are used in a ratio of 3 g: 5 mL: 10 mL: 10 mL: 5 mL: 20 mL, and the precursor, zinc nitrate hexahydrate, deionized water, ammonia water and hydrogen peroxide are used in a ratio of 1 g: 3 g: 20 mL: 1.6 mL: 1.5 mL. Example 3
[0066] A weather-resistant polymer waterproof material for roofing, comprising component A and component B in a mass ratio of 1:2, wherein component A is a modified prepolymer, and component B comprises the following raw materials in parts by weight: 50 parts of polyether 330N, 3 parts of dibutyltin dilaurate, 10 parts of talcum powder, 15 parts of modified filler, 5 parts of methyltrimethoxysilane, 5 parts of dimethyldimethoxysilane, 5 parts of phenyltrimethoxysilane, 3 parts of dispersant, 3 parts of defoamer and 50 parts of xylene;
[0067] The dispersant is 5027 and the defoamer is DF530.
[0068] The modified prepolymer is prepared by the following steps:
[0069] Step S1: 2,2-dihydroxymethylpropionic acid, KH550, dicyclohexylcarbodiimide and toluene are mixed evenly, and reacted at a speed of 300 r / min and a temperature of 50° C. for 5 hours to obtain a chain extension monomer; methyltrifluoropropylcyclotrisiloxane, octamethylcyclotetrasiloxane, tetramethylammonium hydroxide and dimethyl sulfoxide are mixed evenly, and nitrogen is introduced for protection, and reacted at a speed of 150 r / min and a temperature of 95° C. for 4 hours, and then the temperature is raised to 150° C. and kept warm for 1.5 hours to obtain a diamine-terminated polysiloxane;
[0070] Step S2: 2-perfluorooctylethanol, epichlorohydrin, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, tetrabutylammonium bromide and DMF are mixed evenly, nitrogen is introduced for protection, the mixture is reacted for 3 hours at a speed of 150 r / min and a temperature of 120° C., the temperature is lowered to 55° C., sodium hydroxide solution is added, and the mixture is reacted for 8 hours to obtain a modifier, the modifier, diamine-terminated polysiloxane and DMF are mixed evenly, the mixture is reacted for 6 hours at a speed of 200 r / min, a temperature of 25° C. and a pH value of 11 to obtain a waterproof monomer;
[0071] Step S3: uniformly mix the modified monomer, waterproof monomer and polyether 220, introduce nitrogen, stir and add diphenylmethane diisocyanate at a speed of 150 r / min and a temperature of 90°C, react for 3 hours, add a chain extension monomer, and continue to react for 3 hours to obtain a modified prepolymer.
[0072] The molar ratio of 2,2-dihydroxymethylpropionic acid, KH550 and dicyclohexylcarbodiimide in step S1 is 1:1:1.2, and the molar ratio of methyltrifluoropropylcyclotrisiloxane, octamethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and tetramethylammonium hydroxide is 0.5:1.2:3.75:2.5.
[0073] The 2-perfluorooctylethanol, epichlorohydrin, tetrabutylammonium bromide and sodium hydroxide solution described in step S2 are 20mmol:20mmol:0.1g:10mL, the mass fraction of the sodium hydroxide solution is 60%, and the molar ratio of the modifier to the double-terminal polysiloxane is 4:1.
[0074] The molar ratio of the modified monomer, waterproof monomer, polyether 220, diphenylmethane diisocyanate and chain extension monomer described in step S3 is 1:2:5:12:1.
[0075] The modified monomer is prepared by the following steps:
[0076] Step A1: Mix magnesium chips, iodine, 4-bromoanisole and tetrahydrofuran, introduce nitrogen protection, stir for 3 hours at a speed of 150 r / min and a temperature of 70°C, cool to 5°C, add cyanuric chloride, and continue to react for 5 hours to obtain intermediate 1; mix intermediate 1, resorcinol, xylene and cyclopentane sulfone, introduce nitrogen protection, stir and add aluminum chloride at a speed of 150 r / min and a temperature of 90°C, and react for 6 hours to obtain intermediate 2;
[0077] Step A2: The intermediate 2, potassium carbonate, sodium chloroacetate and DMF are mixed evenly, reacted at a speed of 300 r / min and a temperature of 100°C for 8 hours, and then the pH value is adjusted to 6.5 to obtain the intermediate 3. The intermediate 3, diethanolamine, dicyclohexylcarbodiimide and toluene are mixed evenly, reacted at a speed of 150 r / min and a temperature of 120°C for 7 hours to obtain the modified monomer.
[0078] The molar ratio of magnesium chips, iodine, 4-bromoanisole and cyanuric chloride described in step A1 is 50mmol:1mg:50mmol:50mmol, and the molar ratio of intermediate 1, resorcinol and aluminum chloride is 1:2:2.5.
[0079] The usage ratio of intermediate 2, potassium carbonate and sodium chloroacetate in step A2 is 1:2:2, and the molar ratio of intermediate 3, diethanolamine and dicyclohexylcarbodiimide is 1:2:2.1.
[0080] The modified filler is prepared by the following steps:
[0081] Step B1: dissolving nickel nitrate hexahydrate in DMF, stirring and adding aminoterephthalic acid and 2-methylimidazole at a speed of 200 r / min and a temperature of 40° C., stirring for 2 hours, heating to 185° C., reacting for 25 hours to obtain a nickel metal organic framework, and mixing the nickel metal organic framework, KH560 and DMF uniformly, reacting for 7 hours at a speed of 300 r / min, a temperature of 25° C. and a pH value of 11 to obtain a modified nickel framework;
[0082] Step B2: The modified nickel framework, acetonitrile, isopropanol, KH550 and tetraethylammonium hydroxide are mixed evenly, stirred at a speed of 150 r / min and a temperature of 55°C and deionized water is added, and the reaction is carried out for 25 hours to obtain a precursor. The precursor, zinc nitrate hexahydrate and deionized water are mixed evenly, stirred at a speed of 800 r / min and a temperature of 40°C and ammonia water is added. After stirring for 30 minutes, hydrogen peroxide is added, and the reaction is continued for 5 hours to obtain a modified filler.
[0083] The molar ratio of nickel nitrate hexahydrate, aminoterephthalic acid and 2-methylimidazole in step B1 is 2:1:1, and the molar ratio of the amino group on the nickel metal organic framework and KH560 is 1:1.
[0084] The modified nickel framework, acetonitrile, isopropanol, KH550, tetraethylammonium hydroxide and deionized water in step B2 are used in a ratio of 3 g: 5 mL: 10 mL: 10 mL: 5 mL: 20 mL, and the precursor, zinc nitrate hexahydrate, deionized water, ammonia water and hydrogen peroxide are used in a ratio of 1 g: 3 g: 20 mL: 1.6 mL: 1.5 mL.
[0085] Comparative Example 1
[0086] Compared with Example 1, no chain extension monomer was added in this comparative example, and the remaining steps were the same.
[0087] Comparative Example 2
[0088] Compared with Example 1, no waterproof monomer was added in this comparative example, and the remaining steps were the same.
[0089] Comparative Example 3
[0090] Compared with Example 1, no modified monomer was added in this comparative example, and the remaining steps were the same.
[0091] Comparative Example 4
[0092] Compared with Example 1, methyltrimethoxysilane, dimethyldimethoxysilane and phenyltrimethoxysilane were not added in this comparative example, and the remaining steps were the same.
[0093] Comparative Example 5
[0094] Compared with Example 1, this comparative example uses a nickel metal organic framework to replace the modified filler, and the other steps are the same.
[0095] Comparative Example 6
[0096] Compared with Example 1, no modified filler was added in this comparative example, and the remaining steps were the same.
[0097] The waterproof materials prepared in Examples 1-3 and Comparative Examples 1-6 were tested for water impermeability, tensile strength and tensile strength after artificial weathering according to the standard of GB / T16777-2008. According to the standard of GB / T6739-2006, the material thickness was 1.5 mm, the moving speed was 0.5 mm / s, and the pencil hardness was tested. The test results are shown in the following table.
[0098]
[0099] It can be seen from the above table that this application has good weather resistance and water resistance.
[0100] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A weather-resistant polymer waterproof material for roofing, characterized in that: The invention comprises component A and component B in a mass ratio of 1:2, wherein component A is a modified prepolymer, and component B comprises the following raw materials in parts by weight: 40-50 parts of polyether 330N, 1-3 parts of dibutyltin dilaurate, 5-10 parts of talc, 10-15 parts of modified filler, 3-5 parts of methyltrimethoxysilane, 3-5 parts of dimethyldimethoxysilane, 3-5 parts of phenyltrimethoxysilane, 1-3 parts of dispersant, 1-3 parts of defoamer and 30-50 parts of xylene; The modified prepolymer is prepared by the following steps: Step S1: 2,2-dihydroxymethylpropionic acid, KH550, dicyclohexylcarbodiimide and toluene are mixed for reaction to obtain a chain extension monomer, methyltrifluoropropylcyclotrisiloxane, octamethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, tetramethylammonium hydroxide and dimethyl sulfoxide are mixed for reaction, and the temperature is raised and kept to obtain a diamine-terminated polysiloxane; Step S2: 2-perfluorooctylethanol, epichlorohydrin, tetrabutylammonium bromide and DMF are mixed for reaction, the temperature is lowered and a sodium hydroxide solution is added to react to obtain a modifier, and the modifier, diamine-terminated polysiloxane and DMF are mixed for reaction to obtain a waterproof monomer; Step S3: mixing and stirring the modified monomer, the waterproof monomer and the polyether 220, adding diphenylmethane diisocyanate, reacting, adding a chain extension monomer, continuing the reaction, and obtaining a modified prepolymer; The modified monomer is prepared by the following steps: Step A1: After magnesium chips, iodine, 4-bromoanisole and tetrahydrofuran are mixed and stirred, cyanuric chloride is added to cool and the reaction is continued to obtain intermediate 1; intermediate 1, resorcinol, xylene and sulfolane are mixed and stirred, aluminum chloride is added and reacted to obtain intermediate 2; Step A2: After reacting the intermediate 2, potassium carbonate, sodium chloroacetate and DMF, the pH is adjusted to be acidic to obtain the intermediate 3, and the intermediate 3, diethanolamine, dicyclohexylcarbodiimide and toluene are reacted to obtain the modified monomer; The modified filler is prepared by the following steps: Step B1: dissolving nickel nitrate hexahydrate in DMF, stirring, adding aminoterephthalic acid and 2-methylimidazole, stirring, heating and reacting to obtain a nickel metal organic framework, and mixing the nickel metal organic framework, KH560 and DMF to obtain a modified nickel framework; Step B2: The modified nickel framework, acetonitrile, isopropanol, KH550 and tetraethylammonium hydroxide are mixed and stirred, and deionized water is added to react to obtain a precursor. The precursor, zinc nitrate hexahydrate and deionized water are mixed and stirred, and ammonia water is added. After stirring, hydrogen peroxide is added and the reaction is continued to obtain a modified filler.
2. The weather-resistant polymer waterproof material for roofing according to claim 1, characterized in that: The molar ratio of 2,2-dihydroxymethylpropionic acid, KH550 and dicyclohexylcarbodiimide in step S1 is 1:1:1.2, and the molar ratio of methyltrifluoropropylcyclotrisiloxane, octamethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and tetramethylammonium hydroxide is 0.5:1.2:3.75:2.
5.
3. The weather-resistant polymer waterproof material for roofing according to claim 1, characterized in that: The 2-perfluorooctylethanol, epichlorohydrin, tetrabutylammonium bromide and sodium hydroxide solution described in step S2 are 20mmol:20mmol:0.1g:10mL, and the molar ratio of the modifier to the double-terminal polysiloxane is 4:
1.
4. The weather-resistant polymer waterproof material for roofing according to claim 1, characterized in that: The molar ratio of the modified monomer, waterproof monomer, polyether 220, diphenylmethane diisocyanate and chain extension monomer described in step S3 is 1:2:5:12:
1.
5. The weather-resistant polymer waterproof material for roofing according to claim 1, characterized in that: The molar ratio of magnesium chips, iodine, 4-bromoanisole and cyanuric chloride described in step A1 is 50mmol:1mg:50mmol:50mmol, and the molar ratio of intermediate 1, resorcinol and aluminum chloride is 1:2:2.
5.
6. The weather-resistant polymer waterproof material for roofing according to claim 1, characterized in that: The usage ratio of intermediate 2, potassium carbonate and sodium chloroacetate in step A2 is 1:2:2, and the molar ratio of intermediate 3, diethanolamine and dicyclohexylcarbodiimide is 1:2:2.
1.
7. The weather-resistant polymer waterproof material for roofing according to claim 1, characterized in that: The molar ratio of nickel nitrate hexahydrate, aminoterephthalic acid and 2-methylimidazole in step B1 is 2:1:1, and the molar ratio of the amino group on the nickel metal organic framework and KH560 is 1:
1.
8. The weather-resistant polymer waterproof material for roofing according to claim 1, characterized in that: The modified nickel framework, acetonitrile, isopropanol, KH550, tetraethylammonium hydroxide and deionized water in step B2 are used in a ratio of 3 g: 5 mL: 10 mL: 10 mL: 5 mL: 20 mL, and the precursor, zinc nitrate hexahydrate, deionized water, ammonia water and hydrogen peroxide are used in a ratio of 1 g: 3 g: 20 mL: 1.6 mL: 1.5 mL.