A method for preparing SAF from bio-grease

By using a high-active catalyst that uniformly disperses metal nickel on the surface of the indium, zirconium and aluminum composite metal oxide support in a fixed bed reactor, the high energy consumption in the prior art is solved. and complex process problems, efficient and low-cost aviation fuel preparation is achieved and the chemical composition requirements of aviation fuel are met.

CN118580882BActive Publication Date: 2024-11-05LUOYANG HENGJIU BIOENERGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411060294.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-05
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

The existing bioaero fuel preparation methods have problems such as high energy consumption, complicated processes and low catalyst recycling rate, especially the selection and preparation of catalysts have a great impact on product types and quality.

Method used

Using a highly active catalyst for uniformly dispersing metal nickel on the surface of the composite metal oxide support of indium, zirconium and aluminum, the hydrogenation, deoxygenation and cracking are carried out simultaneously in the fixed bed reactor through pretreatment and refining treatment steps, and castor oil is used. Bio-oil esters such as , cicada oil and wood oil are mixed with hydrogen to react to prepare aviation fuel.

Benefits of technology

The bioaero fuel preparation process is simplified, production costs are reduced, yields are improved, excessive production of aromatic hydrocarbons is suppressed, the chemical composition requirements of aviation fuel are met, and the catalyst has good stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118580882B_ABST
    Figure CN118580882B_ABST
Patent Text Reader

Abstract

The present application relates to the field of aviation fuel technology, and specifically discloses a method for preparing SAF from bio-oil. A method for preparing SAF from bio-oil, firstly passing the bio-oil through a pretreatment unit to remove mechanical impurities, phospholipids, chlorine, metals and water, and reduce the oleic acid value, and then passing the bio-oil into a fixed bed reactor loaded with a high-activity catalyst for refining, and fractionating through a fractionation tower to obtain aviation fuel; the high-activity catalyst is: metallic nickel is uniformly dispersed on the surface of a carrier of a composite metal oxide of indium, zirconium and aluminum. The aviation fuel prepared in the present application has hydrocarbons in the category of C8-C16 aviation kerosene, including more alkanes, very small amounts of aromatics and olefins, and has the advantage of meeting the requirements of aviation fuel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of aviation fuel, and more specifically, to a method for preparing SAF from bio-oil. Background Art

[0002] With the increasing concern for the environment and the increasing consumption of fossil fuel resources, biomass, as the main source of renewable energy, has great potential to meet future energy needs. Aviation fuel (SAF) must meet very strict international standards. Its chemical composition is mainly hydrocarbons with carbon chain lengths of C8-C16, mainly containing alkanes, cycloalkanes and aromatic hydrocarbons and a small amount of olefins, among which there are strict restrictions on the content of aromatic hydrocarbons and olefins.

[0003] At present, the bio-aviation fuel preparation methods that are studied more abroad mainly have two-stage hydrogenation processes, the first step: conversion to alkanes on a catalyst, the second step: cracking and isomerization on a suitable catalyst to complete the conversion of crude oil to aviation fuel. Although the two-step process shows a high oil conversion rate and high selectivity for alkanes, it still has the defects of high energy consumption and complicated process. The one-step method for preparing aviation fuel reduces the yield due to the easy generation of a large amount of by-product gas during the production process. Among them, the selection and preparation of the catalyst have the greatest impact on the type and quality of the product. CN113004953A discloses a method for preparing bio-aviation fuel using coconut oil, using a Y-type zeolite molecular sieve, a ZSM-5 zeolite molecular sieve or a ZSM-11 zeolite molecular sieve as a carrier and a modified solid catalyst prepared with ferric oxide-silicon oxide-copper sulfate as an active component, which is successively used in the esterification reaction, hydrodeoxygenation, and isomerization reaction process of coconut oil to obtain bio-aviation fuel; but the preparation process of the bio-aviation fuel is complicated, the energy consumption is high, and the modified solid catalyst needs to be added all the time, and the recycling rate is not high. Summary of the invention

[0004] In order to further improve the efficiency of preparing aviation fuel, the present application provides a method for preparing SAF from bio-oil.

[0005] The present application provides a method for preparing SAF from bio-oil, using the following technical solution:

[0006] A method for preparing SAF from bio-oil comprises the following steps: S1, pretreatment: subjecting the bio-oil to a pretreatment unit to remove mechanical impurities, phospholipids, chlorine, metals and water in the raw material, and to reduce the acid value of the raw material oil, so as to obtain treated bio-oil ester; S2, refining treatment: mixing the treated bio-oil ester and hydrogen and passing it into a fixed bed reactor loaded with a high-activity catalyst for refining, and fractionating it through a fractionation tower to obtain aviation fuel; the bio-oil comprises at least one of castor oil, zelkova oil and wood oil; and the high-activity catalyst comprises: metal nickel uniformly dispersed on the surface of a carrier of a composite metal oxide of indium, zirconium and aluminum.

[0007] By adopting the above technical scheme, a high-activity catalyst with a carrier of a composite metal oxide of indium, zirconium and aluminum and uniformly dispersed metal nickel on the surface is filled in a fixed bed reactor, and bio-oil esters such as castor oil, zelkova oil and wood oil are used as raw materials. After pretreatment, the raw materials are mixed with hydrogen and passed into a fixed bed reactor for refining, thereby achieving simultaneous hydrogenation, deoxygenation and cracking to obtain aviation fuel, avoiding the cumbersome traditional two-step preparation method and reducing production costs.

[0008] Preferably, the pretreatment parameters are set as follows: pressure 6-14 MPa; temperature: 220-380°C; air velocity: 0.5-1.0 h -1 ; Hydrogen to oil volume ratio: (400-800):1.

[0009] By adopting the above technical solution, mechanical impurities, phospholipids, chlorine, metals and water in biological oils can be effectively removed under these conditions, the acid value of the raw oil can be reduced, and the refining requirements can be met.

[0010] Preferably, the refining treatment parameters are set as follows: pressure: 5-14 MPa; temperature: 250-350°C; air velocity: 0.5-1.8 h -1 ; Hydrogen to oil volume ratio: (300-1200):1.

[0011] By adopting the above technical solution, under this condition, the treated bio-oil ester can be fully contacted with the high-activity catalyst on the fixed bed, and the reaction effect is good.

[0012] Preferably, in the refining treatment, the fixed bed reactor loaded with a high-activity catalyst is provided with 2-5 catalyst beds.

[0013] By adopting the above technical solution, under this condition, the treated bio-oil ester can be brought into contact with the high-activity catalyst on the fixed bed for multiple times, and the reaction effect is good.

[0014] Preferably, during the refining treatment, cooling hydrogen facilities are provided between the beds of the fixed bed reactor.

[0015] By adopting the above technical solution, the reaction stability is improved.

[0016] Preferably, the preparation method of the highly active catalyst is as follows: S1, dissolving indium trichloride, zirconium oxychloride, and aluminum chloride in 10 times the mass of deionized water, respectively, and then mixing the three, slowly adding a 40% mass fraction of concentrated ammonia solution under stirring until the pH is 9-10, standing for 24 hours, filtering, repeatedly washing with deionized water until there is no chloride ion, drying at 120-130°C, grinding through a 150-mesh sieve, and then heating to 500-600°C at a rate of 3°C / min in an oxygen atmosphere, sintering for 130-150 minutes, cooling to room temperature, grinding through a 150-mesh sieve, and obtaining a precursor support; S2, immersing the precursor support in a phosphoric acid solution and stirring at room temperature for 12-16 hours. Then the temperature is raised to 70°C, evaporated with stirring, then dried at 100°C overnight, and finally calcined at 430-450°C for 2-3h to obtain a support; S3, the support is immersed in an aqueous solution of nickel nitrate, evaporated and dried overnight, and then calcined at 400-420°C for 3-4h to obtain a precursor catalyst; S4, the precursor catalyst is reduced at 300-350°C in a hydrogen atmosphere for 1.5-2.0h to obtain a highly active catalyst.

[0017] By adopting the above technical scheme, indium, zirconium and aluminum are mixed in a specific proportion, ammonia water is added, oxygen is added for firing, and then phosphoric acid is modified to promote the formation of acid sites on the support. The electronic synergistic effect between nickel oxide and the acid sites on the surface of the support can promote the uniform dispersion of nickel oxide, so that nickel oxide is more conducive to being reduced to highly active nickel element by hydrogen at low temperature. The highly active catalyst acts on bio-oil esters such as castor oil, zelkova oil and wood oil to produce aviation fuel, has a high yield, inhibits excessive production of aromatics, and meets the demand for aviation fuel. At the same time, the highly active catalyst also has quite good stability.

[0018] Preferably, the molar ratio of metal atoms in the indium trichloride, zirconium oxychloride and aluminum chloride is 10-15:20-25:3-8.

[0019] By adopting the above technical solution, the high-activity catalyst prepared under this condition has strong stability.

[0020] Preferably, the mass fraction of the phosphoric acid solution is 0.8-1.2%.

[0021] By adopting the above technical solution, excessive phosphoric acid solution will block the pores of the high-activity catalyst and affect the catalytic activity.

[0022] Preferably, the concentration of the nickel nitrate aqueous solution is 0.1-0.3 g / mL.

[0023] By adopting the above technical solution, if the concentration of the nickel nitrate aqueous solution is too high, nickel oxide will aggregate on the surface of the highly active catalyst, resulting in insufficient reduction and affecting the catalytic activity.

[0024] In summary, this application has the following beneficial effects:

[0025] The present application uses a composite metal oxide support of indium, zirconium, and aluminum and a high-activity catalyst with metal nickel uniformly dispersed on the surface to fill a fixed bed reactor, and uses castor oil, linden oil, wood oil and other bio-oil esters as raw materials. After pretreatment, it is mixed with hydrogen and passed into a fixed bed reactor for refining, realizing the simultaneous hydrogenation, deoxidation, and cracking to obtain aviation fuel, avoiding the cumbersomeness of the traditional two-step preparation method, and reducing production costs. 2. In the present application, indium, zirconium, and aluminum are preferably mixed in a specific ratio, by dripping ammonia water, oxygenating and firing, and then modified by phosphoric acid, and then nickel oxide is loaded on its surface, and reduced by hydrogen to obtain a high-activity catalyst with metal nickel uniformly dispersed on the surface. The high-activity catalyst acts on castor oil, linden oil, wood oil and other bio-oil esters to produce aviation fuel, with a high yield, suppressing the excessive production of aromatics, meeting the needs of aviation fuel, and at the same time, the high-activity catalyst also has quite good stability.

[0026] 3. The aviation fuel prepared by the preparation method of the present application has hydrocarbons in the C8-C16 aviation kerosene range, more alkanes, and very small amounts of aromatics and olefins, meeting the requirements of aviation fuel. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 : SEM and TEM images of the support and high-activity catalyst prepared in Example 2 of the present application, wherein (1) corresponds to the support SEM; (2) corresponds to the high-activity catalyst SEM; (3) corresponds to the support TEM; (4) corresponds to the high-activity catalyst SEM.

[0028] Figure 2 : XRD diagram of the support and high-activity catalyst prepared in Example 2 of the present application, wherein the upper curve is the high-activity catalyst and the lower curve is the support. DETAILED DESCRIPTION

[0029] The present application is further described in detail below in conjunction with embodiments.

[0030] Unless otherwise specified, the raw materials used in the examples and comparative examples of the present application are all commercially available.

[0031] Example

[0032] Example 1

[0033] A method for preparing SAF from bio-grease comprises the following steps:

[0034] S1, pretreatment: the bio-oil is passed through the pretreatment unit to remove mechanical impurities, phospholipids, chlorine, metals and water in the raw material, and the acid value of the raw material oil is reduced to obtain the treated bio-oil ester. The pretreatment parameters are set as follows: pressure 6MPa; temperature: 220℃; air velocity: 0.5h -1 ; Hydrogen oil volume ratio: 400:1;

[0035] S2, refining treatment: the treated bio-oil ester and hydrogen are mixed and passed into a fixed bed reactor loaded with a high-activity catalyst for refining, and then fractionated through a fractionation tower to obtain aviation fuel. The refining treatment parameters are set as follows: pressure: 5MPa; temperature: 250℃; space velocity: 0.5h -1 ; Hydrogen-oil volume ratio: 300:1. The fixed bed reactor loaded with high-activity catalyst is equipped with 5 catalyst beds, and cooling hydrogen facilities are installed between the beds of the fixed bed reactor.

[0036] The biological oil is catalpa oil.

[0037] The preparation method of the highly active catalyst is as follows:

[0038] S1, dissolve 1.5g of indium trichloride, 2.4g of zirconyl chloride, and 0.27g of aluminum chloride in 10 times the mass of deionized water (the molar ratio of metal atoms in indium trichloride, zirconyl chloride, and aluminum chloride is 10:20:3), then mix the three, slowly add 40% by mass concentrated ammonia solution under stirring until the pH is 9, let stand for 24 hours, filter, repeatedly wash with deionized water until there is no chloride ion, dry at 120°C, grind through a 150-mesh sieve, and then heat to 500°C at a rate of 3°C / min in an oxygen atmosphere, sinter for 130 minutes, cool to room temperature, grind through a 150-mesh sieve, and obtain a precursor support;

[0039] S2, immerse the precursor support in a 0.8% phosphoric acid solution, stir at room temperature for 12 hours, then heat to 70°C, stir and evaporate to dryness, then dry at 100°C overnight, and finally calcine at 430°C for 2 hours to obtain the support;

[0040] S3, immersing the support in a nickel nitrate aqueous solution, evaporating and drying overnight, and then calcining at 400° C. for 3 h to obtain a precursor catalyst;

[0041] S4, reducing the precursor catalyst at 300° C. for 1.5 h in a hydrogen atmosphere to obtain a highly active catalyst, wherein the concentration of the nickel nitrate aqueous solution is 0.1 g / mL.

[0042] Example 2

[0043] A method for preparing SAF from bio-grease comprises the following steps:

[0044] S1, pretreatment: the bio-oil is passed through the pretreatment unit to remove mechanical impurities, phospholipids, chlorine, metals and water in the raw material, and the acid value of the raw material oil is reduced to obtain the treated bio-oil ester. The pretreatment parameters are set as follows: pressure 8MPa; temperature: 250℃; air velocity: 0.8h -1 ; Hydrogen oil volume ratio: 600:1;

[0045] S2, refining treatment: the treated bio-oil ester and hydrogen are mixed and passed into a fixed bed reactor loaded with a high-activity catalyst for refining, and then fractionated through a fractionation tower to obtain aviation fuel. The refining treatment parameters are set as follows: pressure: 10MPa; temperature: 300℃; space velocity: 1.2h -1 ; Hydrogen-oil volume ratio: 800:1. The fixed bed reactor loaded with high-activity catalyst is equipped with 3 catalyst beds, and cooling hydrogen facilities are installed between the beds of the fixed bed reactor.

[0046] The biological oil is castor oil.

[0047] The preparation method of the highly active catalyst is as follows:

[0048] S1, dissolve 2.0g of indium trichloride, 2.96g of zirconyl chloride, and 0.5g of aluminum chloride in 10 times the mass of deionized water (the molar ratio of metal atoms in indium trichloride, zirconyl chloride, and aluminum chloride is 12:22:5), then mix the three, slowly drop 40% concentrated ammonia solution under stirring until the pH is 10, let stand for 24h, filter, repeatedly wash with deionized water until there is no chloride ion, dry at 125°C, grind through a 150-mesh sieve, and then heat to 550°C at a rate of 3°C / min in an oxygen atmosphere, sinter for 140min, cool to room temperature, grind through a 150-mesh sieve, and obtain a precursor support;

[0049] S2, immerse the precursor support in a 0.9% phosphoric acid solution, stir at room temperature for 14 hours, then heat to 70°C, stir and evaporate to dryness, then dry at 100°C overnight, and finally calcine at 440°C for 2.5 hours to obtain the support;

[0050] S3, immersing the support in a nickel nitrate aqueous solution, evaporating and drying overnight, and then calcining at 410° C. for 3.5 h to obtain a precursor catalyst;

[0051] S4, reducing the precursor catalyst at 340° C. for 2.0 h in a hydrogen atmosphere to obtain a highly active catalyst, wherein the concentration of the nickel nitrate aqueous solution is 0.2 g / mL.

[0052] Scanning electron microscopy was used to observe the surface structure of the support and highly active catalysts, e.g. Figure 1 (1) and (2); transmission electron microscopy was used to observe the pore structure of the support and the highly active catalyst, such as Figure 1in (3) and (4).

[0053] from Figure 1 It can be seen from (1) and (2) that the surface of the support body presents a flaky crystal structure, the flaky crystals are tightly connected, and the surface is relatively smooth and flat; the surface of the high-activity catalyst is still a flaky structure, but the difference is that the surface becomes rough, and there are small particles evenly dispersed on the surface, which may be the supported metal nickel.

[0054] from Figure 1 As can be seen in (3) and (4), the crystals of the support are close to elliptical, and the pore size is uniform, about 12-18nm. The metal nickel particles are evenly dispersed on the surface of the high-activity catalyst, and the pore structure of the high-activity catalyst is reduced and smaller, with a pore size of about 10-14nm.

[0055] The crystal structures of the supports and highly active catalysts were determined using X-ray diffractometers, such as Figure 2 As shown, Figure 2 The upper middle curve is a highly active catalyst, and the lower curve is a support.

[0056] from Figure 2 It can be seen that the diffraction peaks of the support and the highly active catalyst are similar, and the crystal structure of the support remains intact after the metal is loaded, indicating that the loading of the metal does not have much effect on the structure and properties of the support catalyst. The diffraction peaks at 2θ=44.5° and 51.8° indicate that nickel oxide is reduced to metallic nickel during the reduction process.

[0057] Example 3

[0058] A method for preparing SAF from bio-grease comprises the following steps:

[0059] S1, pretreatment: The bio-oil is passed through a pretreatment unit to remove mechanical impurities, phospholipids, chlorine, metals and water in the raw material, and the acid value of the raw material oil is reduced to obtain treated bio-oil ester. The pretreatment parameters are set as follows: pressure 14MPa; temperature: 380℃; air velocity: 1.0h -1 ; Hydrogen oil volume ratio: 800:1;

[0060] S2, refining treatment: the treated bio-oil ester and hydrogen are mixed and passed into a fixed bed reactor loaded with a high-activity catalyst for refining, and then fractionated through a fractionation tower to obtain aviation fuel. The refining treatment parameters are set as follows: pressure: 14MPa; temperature: 350℃; space velocity: 1.8h -1 ; Hydrogen-oil volume ratio: 1200:1. The fixed bed reactor loaded with high-activity catalyst is equipped with two catalyst beds, and a cooling hydrogen facility is provided between the beds of the fixed bed reactor.

[0061] The biological oil is wood oil.

[0062] The preparation method of the highly active catalyst is as follows:

[0063] S1, 3.0g of indium trichloride, 4.0g of zirconyl chloride, and 0.96g of aluminum chloride are dissolved in 10 times the mass of deionized water (the molar ratio of metal atoms in indium trichloride, zirconyl chloride, and aluminum chloride is 15:25:8, and then the three are mixed, and a 40% mass fraction of concentrated ammonia solution is slowly added dropwise under stirring until the pH is 10, and the mixture is allowed to stand for 24 hours, filtered, and repeatedly washed with deionized water until there is no chloride ion, dried at 130°C, ground through a 150-mesh sieve, and then heated to 600°C at a rate of 3°C / min in an oxygen atmosphere, fired for 150 minutes, cooled to room temperature, and ground through a 150-mesh sieve to obtain a precursor support;

[0064] S2, immerse the precursor support in a 1.2% phosphoric acid solution, stir at room temperature for 16 hours, then heat to 70°C, evaporate to dryness with stirring, then dry at 100°C overnight, and finally calcine at 450°C for 3 hours to obtain the support;

[0065] S3, immersing the support in a nickel nitrate aqueous solution, evaporating and drying overnight, and then calcining at 420° C. for 4 h to obtain a precursor catalyst;

[0066] S4, reducing the precursor catalyst at 350° C. for 2.0 h in a hydrogen atmosphere to obtain a highly active catalyst, wherein the concentration of the nickel nitrate aqueous solution is 0.3 g / mL.

[0067] Comparative Example

[0068] Comparative Example 1

[0069] The method is the same as Example 2, except that the high-activity catalyst is not immersed in phosphoric acid during preparation, that is, step S2 is not performed, and the precursor support in step S1 is directly subjected to step S3 to prepare the catalyst.

[0070] Comparative Example 2

[0071] The same as Example 2, except that during the preparation of the high-activity catalyst, the molar ratio of metal atoms in indium trichloride, zirconium oxychloride and aluminum chloride was adjusted to 1:1:1; that is, 3.0 g indium trichloride, 2.4 g zirconium oxychloride and 1.8 g aluminum chloride.

[0072] Comparative Example 3

[0073] The same as Example 2, except that during the preparation of the high-activity catalyst, the concentration of the nickel nitrate aqueous solution was 0.5 g / mL.

[0074] Comparative Example 4

[0075] The same as Example 2, except that during the preparation of the high-activity catalyst, the calcination temperature of step S1 was adjusted to 700°C.

[0076] Performance testing

[0077] 1. The iodine value, oxygen content and carbon number distribution of the aviation fuel prepared in Example 2 and Comparative Examples 1-4 were tested. The results are shown in Table 1. In addition, the iodine value of the castor oil raw material used was measured to be 85%, the oxygen content was 15.3%, and the H / C ratio was 1.89.

[0078] Table 1. Test results of aviation fuel

[0079]

[0080] As can be seen from Table 1, the iodine value of the aviation fuel prepared by using the high-activity catalyst prepared in Example 2 of the present application to act on bio-oil ester castor oil is low, which shows that the high-activity catalyst prepared in Example 2 has strong catalytic hydrogenation performance, low oxygen content and significantly reduced H / C ratio, indicating that the high-activity catalyst prepared in Example 2 performs hydrogenation, cracking and deoxygenation simultaneously. From the perspective of overall catalytic performance, Example 2 and Comparative Example 2 have the best use effect.

[0081] 2. The high-activity catalysts prepared in Example 2 and Comparative Example 2 were washed and dried with n-hexane, and then calcined again at 410°C for 3.5 hours, and then reduced at 340°C for 2.0 hours in a hydrogen atmosphere to remove the carbon deposited on the surface of the high-activity catalysts, activated and regenerated, and aviation fuel was prepared again, and this was repeated twice. The stability of the high-activity catalysts was analyzed and evaluated.

[0082] Table 2. High activity catalyst stability test

[0083]

[0084] It can be seen from Table 2 that, compared with Comparative Example 2, the high-activity catalyst prepared in Example 2 of the present application has excellent stability and can be recycled, and the main component categories of the prepared aviation fuel have not changed significantly.

[0085] 3. The properties of the aviation fuel prepared in Example 2 were tested, and the results are shown in Table 3:

[0086] Table 3. Aviation fuel properties test

[0087]

[0088] It can be seen from Table 3 that the aviation fuel prepared in Example 2 of the present application meets all the indicators under HEFA SPK required by ASTM D7566 standard.

[0089] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, a person skilled in the art may make non-creative modifications to the present embodiment as needed, and such modifications shall be protected by the patent law as long as they are within the scope of protection claimed in the present application.

Claims

1. A method for preparing SAF from bio-oil, characterized in that: The following steps are involved: S1, pretreatment: the bio-oil is passed through a pretreatment unit to remove mechanical impurities, phospholipids, chlorine, metals and water in the raw material, and the acid value of the raw material oil is reduced to obtain treated bio-oil ester; S2, refining treatment: the treated bio-oil ester and hydrogen are mixed and passed into a fixed bed reactor loaded with a high-activity catalyst for refining, and then fractionated through a fractionation tower to obtain aviation fuel; the bio-oil includes at least one of castor oil, linden oil and wood oil; the high-activity catalyst is: metal nickel is uniformly dispersed on the surface of a composite metal oxide support of indium, zirconium and aluminum; The preparation method of the high-activity catalyst is as follows: S1, dissolving indium trichloride, zirconium oxychloride and aluminum chloride in 10 times the mass of deionized water respectively, then mixing the three, slowly dropping a 40% by mass concentrated ammonia solution under stirring until the pH value is 9-10, standing for 24 hours, filtering, repeatedly washing with deionized water until there is no chloride ion, drying at 120-130°C, grinding through a 150-mesh sieve, and then heating to 500-600°C at a rate of 3°C / min in an oxygen atmosphere, calcining for 130-150 minutes, cooling to room temperature, grinding through a sieve of 150 meshes ... and grinding through a sieve of 150 meshes. 150 mesh sieve to obtain a precursor support; S2, immerse the precursor support in a phosphoric acid solution, stir at room temperature for 12-16 hours, then heat to 70°C, evaporate to dryness with stirring, then dry at 100°C overnight, and finally calcine at 430-450°C for 2-3 hours to obtain a support; S3, immerse the support in a nickel nitrate aqueous solution, evaporate to dryness and dry overnight, and then calcine at 400-420°C for 3-4 hours to obtain a precursor catalyst; S4, reduce the precursor catalyst at 300-350°C in a hydrogen atmosphere for 1.5-2.0 hours to obtain a highly active catalyst; The molar ratio of metal atoms in the indium trichloride, zirconium oxychloride and aluminum chloride is 10-15:20-25:3-8; The concentration of the nickel nitrate aqueous solution is 0.1-0.3 g / mL.

2. The method for preparing SAF from bio-oil according to claim 1, characterized in that: The pretreatment parameters are set as follows: pressure 6-14MPa; temperature: 220-380℃; air velocity: 0.5-1.0h -1 ; Hydrogen to oil volume ratio: (400-800):

1.

3. The method for preparing SAF from bio-oil according to claim 2, characterized in that: The refining treatment parameters are set as follows: pressure: 5-14MPa; Temperature: 250-350℃; air speed: 0.5-1.8h -1 ; Hydrogen to oil volume ratio: (300-1200):

1.

4. The method for preparing SAF from bio-oil according to claim 3, characterized in that: During the refining treatment, a fixed bed reactor loaded with a high-activity catalyst is provided with 2-5 catalyst beds.

5. The method for preparing SAF from bio-oil according to claim 4, characterized in that: During the refining process, cooling hydrogen facilities are installed between the beds of the fixed bed reactor.

6. The method for preparing SAF from bio-oil according to claim 5, characterized in that: The mass fraction of the phosphoric acid solution is 0.8-1.2%.