Ganoderma lucidum mycelium leather and preparation method thereof

Through the deacetylation treatment of Ganoderma lucidum mycelium tablets and the hot pressing treatment in the cross-linking solution, chemical cross-linking and hydrogen bonds are formed by using organic polycarboxylic acids and polyvinyl alcohol to form, the leather mechanics of Ganoderma lucidum mycelium in the prior art were solved. The problem of insufficient performance significantly improves the mechanical properties and stability of the material.

CN118581742BActive Publication Date: 2024-11-19SHANGHAI HEXIANG HEALTH TECH DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411052834.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19
Estimated Expiration
2044-08-02

AI Technical Summary

Technical Problem

In the prior art, it is difficult to significantly improve the mechanical properties of Ganoderma lucidum mycelium leather by reacting a single chemical crosslinking agent with the deacetylated mycelium tablets, resulting in the phenomenon of tearing and breaking of the leather.

Method used

The deacetylation-treated Ganoderma lucidum mycelium tablets are heat-pressed in the cross-linking solution, and chemical cross-linking and hydrogen bonding are used to form with organic polycarboxylic acid and polyvinyl alcohol (PVA), which improves the mechanical properties of Ganoderma lucidum mycelium leather.

Benefits of technology

Through the synergistic action of chemical crosslinking and hydrogen bonding, the mechanical properties of Ganoderma lucidum mycelium leather are significantly improved, and the tearing and damage of the leather is avoided, and the stability and strength of the material are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention belongs to the technical field of leather preparation, and provides a ganoderma lucidum hyphae leather and a preparation method thereof. The present invention performs deacetylation treatment on ganoderma lucidum hyphae sheets, which can expose amino groups on the ganoderma lucidum hyphae sheets, and provide active sites for subsequent chemical crosslinking. The present invention soaks the deacetylated hyphae sheets in a crosslinking solution (including organic polycarboxylic acids and polyvinyl alcohol). During the soaking process, the organic polycarboxylic acids and polyvinyl alcohol in the crosslinking solution are fully impregnated into the deacetylated hyphae sheets; during the hot pressing process, the organic polycarboxylic acids impregnated into the deacetylated hyphae sheets are chemically crosslinked with the hydroxyl groups and amino groups on the ganoderma lucidum hyphae sheets; the hydroxyl groups of the polyvinyl alcohol can form stable hydrogen bonds with the hydroxyl groups on the deacetylated hyphae sheets; the combination of chemical crosslinking and stable hydrogen bonds improves the mechanical properties of the ganoderma lucidum hyphae leather.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of leather preparation, in particular to ganoderma lucidum mycelium leather and a preparation method thereof. Background Art

[0002] Ganoderma lucidum mycelium leather is a kind of soft material made from mycelium produced by solid-state fermentation or liquid-state fermentation of Ganoderma lucidum. In order to improve the mechanical properties of Ganoderma lucidum mycelium leather materials, they must be cross-linked. The commonly used cross-linking method is to add cross-linking agents such as glutaraldehyde, dicarboxylic acid, tricarboxylic acid, and tannin, so that these cross-linking agents react with the chitosan amino groups in the deacetylated mycelium sheets to form interchain cross-links and improve the mechanical properties of Ganoderma lucidum mycelium leather materials. However, the mass fraction of chitosan amino groups in the deacetylated mycelium sheets only accounts for 8% to 12% of the total. The Ganoderma lucidum mycelium leather materials obtained only by single chemical cross-linking still cannot meet the mechanical performance requirements, and the finished leather is prone to tearing and damage. Summary of the invention

[0003] In view of this, the object of the present invention is to provide a ganoderma lucidum mycelium leather and a preparation method thereof. The ganoderma lucidum mycelium leather obtained by the preparation method provided by the present invention has high mechanical properties.

[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0005] The present invention provides a method for preparing ganoderma lucidum mycelium leather, comprising the following steps:

[0006] Deacetylation of the ganoderma mycelium slices is performed to obtain deacetylated mycelium slices;

[0007] After soaking the deacetylated mycelium sheet in a cross-linking solution, hot pressing is performed to obtain the Ganoderma lucidum mycelium leather;

[0008] The cross-linking solution includes organic polycarboxylic acid and polyvinyl alcohol (PVA).

[0009] Preferably, the method for preparing the Ganoderma lucidum mycelium slice comprises the following steps:

[0010] The liquid fermented ganoderma mycelium is dispersed in water, and the water is removed by suction filtration and pressed in sequence to obtain the ganoderma mycelium slices.

[0011] Preferably, the reagent for the deacetylation treatment is an inorganic alkali solution, the inorganic alkali in the inorganic alkali solution includes one or more of sodium hydroxide, calcium hydroxide and sodium bicarbonate, and the mass fraction of the inorganic alkali in the inorganic alkali solution is 1-16%.

[0012] Preferably, the deacetylation treatment is carried out at a temperature of 45-95° C. and for a time of 1-20 h.

[0013] Preferably, in the cross-linking solution, the mass fraction of the organic polycarboxylic acid is 3-5%, and the mass fraction of the polyvinyl alcohol is 2-10%;

[0014] The organic polycarboxylic acid includes one or more of citric acid, succinic acid, adipic acid and butanetetracarboxylic acid.

[0015] Preferably, the molecular weight of the polyvinyl alcohol is 500-2000 Da.

[0016] Preferably, the soaking temperature is 20-60° C. and the soaking time is 2-12 hours.

[0017] Preferably, after the soaking and before the hot pressing, the method further comprises: taking out the soaked mycelium sheets and drying them, wherein the drying temperature is 45-85°C.

[0018] Preferably, the hot pressing temperature is 100-150° C., the pressure is 1.5-9 MPa, and the heat preservation and pressure holding time is 5-180 min.

[0019] The present invention also provides ganoderma lucidum mycelium leather obtained by the preparation method described in the above technical scheme.

[0020] The deacetylation treatment of the ganoderma mycelium sheet by the present invention can expose the amino groups on the ganoderma mycelium sheet, providing active sites for subsequent chemical crosslinking. The present invention places the deacetylated mycelium sheet in a crosslinking solution (including organic polycarboxylic acid and polyvinyl alcohol), and during the soaking process, the organic polycarboxylic acid and polyvinyl alcohol in the crosslinking solution are fully impregnated into the deacetylated mycelium sheet; during the hot pressing process, the organic polycarboxylic acid impregnated into the deacetylated mycelium sheet is chemically crosslinked with the hydroxyl group and the amino group on the ganoderma mycelium sheet; the hydroxyl group of the polyvinyl alcohol forms a stable hydrogen bond with the hydroxyl group on the deacetylated mycelium sheet; the combination of chemical crosslinking and stable hydrogen bonding improves the mechanical properties of the ganoderma mycelium leather. DETAILED DESCRIPTION

[0021] The present invention provides a method for preparing ganoderma lucidum mycelium leather, comprising the following steps:

[0022] Deacetylation of the ganoderma mycelium slices is performed to obtain deacetylated mycelium slices;

[0023] After soaking the deacetylated mycelium sheet in a cross-linking solution, hot pressing is performed to obtain the Ganoderma lucidum mycelium leather;

[0024] The cross-linking solution includes organic polycarboxylic acid and polyvinyl alcohol.

[0025] In the present invention, unless otherwise specified, the raw materials used in the present invention are preferably commercially available products.

[0026] The invention carries out deacetylation treatment on the ganoderma lucidum mycelium slices to obtain deacetylated mycelium slices.

[0027] In the present invention, the method for preparing the Ganoderma lucidum mycelium slice preferably comprises the following steps:

[0028] The liquid fermented ganoderma mycelium is dispersed in water, and the water is removed by suction filtration and pressed in sequence to obtain the ganoderma mycelium slices.

[0029] In the present invention, the liquid fermented Ganoderma lucidum mycelium is preferably a commercially available product, and more preferably the liquid fermented Ganoderma lucidum mycelium purchased from Shanghai Hexiang Health Technology Development Co., Ltd. In the present invention, the dispersion is preferably carried out under stirring. In the present invention, the dosage ratio of the liquid fermented Ganoderma lucidum mycelium and water is preferably 5~20g:200~1000mL, and more preferably 10g:500mL. The present invention does not specifically limit the method of filtering and removing water, and means familiar to those skilled in the art can be used. In the present invention, the pressure of the pressing treatment is preferably 3~15kPa, and more preferably 6~12kPa, and the time is preferably 1~10min. In the present invention, the water content of the Ganoderma lucidum mycelium sheet is preferably 50~80%.

[0030] In the present invention, the deacetylation reagent is preferably an inorganic alkali solution, and the inorganic alkali in the inorganic alkali solution preferably includes one or more of sodium hydroxide, calcium hydroxide and sodium bicarbonate, and more preferably sodium hydroxide. In the present invention, the mass fraction of the inorganic alkali in the inorganic alkali solution is preferably 1-16%, and more preferably 4-12%.

[0031] In the present invention, the deacetylation treatment preferably comprises: immersing the Ganoderma lucidum mycelium sheet in a deacetylation treatment reagent.

[0032] In the present invention, the temperature of the deacetylation treatment is preferably 45-95°C, more preferably 50-90°C, more preferably 60-80°C, and most preferably 70°C; the time is preferably 1-20h, more preferably 5-15h.

[0033] After the deacetylation treatment, the present invention preferably further comprises: removing the material and washing it with water. The present invention does not specifically limit the amount and number of reagents for the washing, as long as the material can be washed to neutrality.

[0034] In the present invention, the deacetylation treatment can expose the amino groups on the Ganoderma lucidum mycelium sheets, provide active sites for subsequent chemical cross-linking, thereby improving the cross-linking strength of the Ganoderma lucidum mycelium, and ultimately improving the mechanical strength of the Ganoderma lucidum mycelium leather.

[0035] After obtaining the deacetylated mycelium sheet, the present invention soaks the deacetylated mycelium sheet in a cross-linking solution and then performs hot pressing to obtain the ganoderma lucidum mycelium leather.

[0036] In the present invention, the cross-linking solution comprises an organic polycarboxylic acid and polyvinyl alcohol. In the present invention, the organic polycarboxylic acid preferably comprises one or more of citric acid, succinic acid, adipic acid and butanetetracarboxylic acid, more preferably citric acid. In the present invention, the molecular weight of the polyvinyl alcohol is preferably 500-2000Da, more preferably 1000-1500Da.

[0037] In the present invention, in the cross-linking solution, the mass fraction of the organic polycarboxylic acid is preferably 3-5%, more preferably 3.5-4.5%, and more preferably 4%; the mass fraction of the polyvinyl alcohol is preferably 2-10%, more preferably 3-9%, more preferably 4-8%, and most preferably 5-7%.

[0038] In the present invention, the soaking temperature is preferably 20-60°C, more preferably 30-50°C, and more preferably 40°C; and the soaking time is preferably 2-12 hours.

[0039] After the soaking and before the hot pressing, the present invention preferably further comprises: drying the soaked mycelium pieces. In the present invention, the drying temperature is preferably 45-85°C, more preferably 50-70°C, and more preferably 55-65°C.

[0040] In the present invention, the deacetylated mycelium sheet is immersed in a cross-linking solution, so that the organic polycarboxylic acid and polyvinyl alcohol in the cross-linking solution can be fully impregnated into the deacetylated mycelium sheet, and PVA can introduce a large number of hydroxyl groups, which can form effective hydrogen bonds with the hydroxyl groups on chitosan in the Ganoderma lucidum mycelium sheet during subsequent hot pressing; at the same time, the carboxyl groups in the organic polycarboxylic acid can chemically cross-link with the hydroxyl groups and amino groups on chitosan during the hot pressing process; effective hydrogen bonds and traditional chemical cross-linking work together to greatly improve the mechanical properties of Ganoderma lucidum mycelium leather. At the same time, when the molecular weight of PVA is within the range of 500~2000Da, effective hydrogen bond cross-linking can be formed between chitosan and PVA, and the mechanical properties of the finished leather are excellent (see Examples 1~3); when the molecular weight of PVA is less than 500Da, the molecular volume of PVA is insufficient, and it is difficult to form hydrogen bonds with chitosan, and the mechanical properties of the finished leather are poor (see Comparative Example 1); when the molecular weight of PVA is greater than 2000Da, PVA is difficult to penetrate into the mycelium sheet, resulting in poor mechanical properties of the final leather (see Comparative Example 2).

[0041] In the present invention, the hot pressing temperature is preferably 100-150°C, more preferably 110-140°C, and more preferably 120-130°C; the pressure is preferably 1.5-9MPa, more preferably 3-7.5MPa, and more preferably 4.5-6MPa; the heat preservation and pressure holding time is preferably 5-180min, and more preferably 30-150min.

[0042] In the present invention, during the hot pressing process, the hydroxyl groups in PVA and the hydroxyl groups on the Ganoderma lucidum mycelium sheet can form effective hydrogen bonds; the hydroxyl groups and amino groups on the chitosan in the deacetylated mycelium sheet can also be chemically cross-linked with the organic polycarboxylic acid.

[0043] The present invention also provides ganoderma lucidum mycelium leather obtained by the preparation method described in the above technical scheme.

[0044] The ganoderma mycelium leather and the preparation method thereof provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0045] Liquid fermented Ganoderma lucidum mycelium was purchased from Shanghai Hexiang Health Technology Development Co., Ltd.

[0046] Example 1

[0047] Preparation of Ganoderma lucidum mycelium slices: The steps are as follows: disperse 10 g of liquid fermented Ganoderma lucidum mycelium in 500 mL of water under stirring, then filter to remove water, and then press at 9 kPa for 5 minutes to obtain Ganoderma lucidum mycelium slices with a water content of 60%.

[0048] Deacetylation treatment: The Ganoderma lucidum mycelium slices were immersed in a 4 wt % NaOH aqueous solution at 70° C. for 8 h for deacetylation treatment. Afterwards, the surface of the Ganoderma lucidum mycelium slices was rinsed with water until neutral to obtain deacetylated mycelium slices.

[0049] Soaking: Soak the deacetylated mycelium sheet in a mixed aqueous solution of 4wt% citric acid and 6wt% PVA (molecular weight 500Da) at 40°C for 3h to allow the PVA molecules to fully penetrate into the deacetylated mycelium sheet; place the soaked deacetylated mycelium sheet in a forced air drying oven at 65°C for drying to obtain a leather precursor.

[0050] Hot pressing: The leather precursor is hot pressed at 4.5 MPa and 120°C for 1 hour to allow the hydroxyl groups in the chitosan to form hydrogen bonds with the PVA to cross-link, thus obtaining the Ganoderma lucidum mycelium leather.

[0051] Example 2

[0052] The only difference from Example 1 is that the molecular weight of PVA is 1000 Da, and the rest is the same as Example 1.

[0053] Example 3

[0054] The only difference from Example 1 is that the molecular weight of PVA is 1500 Da, and the rest is the same as Example 1.

[0055] Example 4

[0056] The only difference from Example 1 is that the molecular weight of PVA is 2000Da, and the rest is the same as Example 1.

[0057] Example 5

[0058] The only difference from Example 1 is that the reagent for deacetylation treatment is replaced by a sodium hydroxide solution with a mass fraction of 16%, and the rest is the same as Example 1.

[0059] Example 6

[0060] The only difference from Example 1 is that the reagent for deacetylation treatment is replaced by a calcium hydroxide solution with a mass fraction of 4%, and the rest is the same as Example 1.

[0061] Example 7

[0062] The only difference from Example 1 is that the reagent for deacetylation treatment is replaced by a sodium bicarbonate solution with a mass fraction of 4%, and the rest is the same as Example 1.

[0063] Example 8

[0064] The only difference from Example 1 is that the mass fraction of citric acid in the cross-linking solution is adjusted to 3%, and the rest is the same as Example 1.

[0065] Example 9

[0066] The only difference from Example 1 is that the mass fraction of citric acid in the cross-linking solution is adjusted to 5%, and the rest is the same as Example 1.

[0067] Example 10

[0068] The only difference from Example 1 is that the citric acid in the cross-linking solution is replaced by succinic acid, and the rest is the same as Example 1.

[0069] Comparative Example 1

[0070] The only difference from Example 1 is that the molecular weight of PVA is 300 Da, and the rest is the same as Example 1.

[0071] Comparative Example 2

[0072] The only difference from Example 1 is that the molecular weight of PVA is 2500 Da, and the rest is the same as Example 1.

[0073] Comparative Example 3

[0074] The only difference from Example 1 is that PVA is replaced by PEG, and the rest is the same as Example 1.

[0075] Comparative Example 4

[0076] The only difference from Example 1 is that PVA is not added, and the rest is the same as Example 1.

[0077] The mechanical properties of the obtained mycelium leather were tested using QB / T 2710-2018 and QB / T 2714-2018, and the results are shown in Table 1.

[0078] Table 1 Mechanical properties test results of Ganoderma lucidum mycelium leather obtained in Examples and Comparative Examples

[0079]

[0080] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing ganoderma lucidum mycelium leather, characterized in that: The following steps are involved: Deacetylation of the ganoderma mycelium slices is performed to obtain deacetylated mycelium slices; After soaking the deacetylated mycelium sheet in a cross-linking solution, hot pressing is performed to obtain the Ganoderma lucidum mycelium leather; The cross-linking solution includes organic polycarboxylic acid and polyvinyl alcohol; The molecular weight of the polyvinyl alcohol is 500-2000Da; The method for preparing the ganoderma lucidum mycelium tablet comprises the following steps: The liquid fermented ganoderma mycelium is dispersed in water, and the water is removed by suction filtration and pressed in sequence to obtain the ganoderma mycelium slices.

2. The preparation method according to claim 1, characterized in that: The reagent for the deacetylation treatment is an inorganic alkali solution, the inorganic alkali in the inorganic alkali solution includes one or more of sodium hydroxide, calcium hydroxide and sodium bicarbonate, and the mass fraction of the inorganic alkali in the inorganic alkali solution is 1-16%.

3. The preparation method according to claim 1 or 2, characterized in that: The temperature of the deacetylation treatment is 45-95° C. and the time is 1-20 hours.

4. The preparation method according to claim 1, characterized in that: In the cross-linking solution, the mass fraction of the organic polycarboxylic acid is 3-5%, and the mass fraction of the polyvinyl alcohol is 2-10%; The organic polycarboxylic acid includes one or more of citric acid, succinic acid, adipic acid and butanetetracarboxylic acid.

5. The preparation method according to claim 1 or 4, characterized in that: The soaking temperature is 20°C to 60°C, and the soaking time is 2 to 12 hours.

6. The preparation method according to claim 1, characterized in that: After the soaking and before the hot pressing, the method further comprises: drying the soaked mycelium sheets at a temperature of 45-85°C.

7. The preparation method according to claim 1, characterized in that: The hot pressing temperature is 100-150° C., the pressure is 1.5-9 MPa, and the heat preservation and pressure holding time is 5-180 min.

8. Ganoderma lucidum mycelium leather obtained by the preparation method according to any one of claims 1 to 7.