Solid electrolyte, secondary battery, preparation method thereof, and electrical device

By using inorganic fillers and coupling agents to form solid electrolytes in the porous structure of the porous support membrane, the problem of insufficient binding force and compatibility in the solid electrolyte membrane is solved, the electrochemical performance and stability are improved, and the secondary battery is improved overall performance.

CN118589023BActive Publication Date: 2024-11-19SONGSHAN LAKE MATERIALS LAB +1
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202411074014.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-19
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The lack of binding force and compatibility between the porous support membrane and the electrolyte in the existing solid electrolyte membrane has affected the structural stability and electrochemical performance of the solid electrolyte membrane, especially the electrode/solid electrolyte interface problem has not been effectively solved.

Method used

Using a combination of porous support film, inorganic filler and coupling agent, solid electrolyte is formed in the porous support film through in situ polymerization technology to improve its ionic conductivity and mechanical strength, and to improve the between inorganic filler and polymer. Interface bonding power.

Benefits of technology

It significantly improves the structural stability and electrochemical performance of solid electrolytes, including cycle stability and high voltage resistance, reduces the interface resistance of the secondary battery during charging and discharging, and improves energy density and safety performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118589023B_ABST
    Figure CN118589023B_ABST
Patent Text Reader

Abstract

The present application relates to a solid electrolyte, a secondary battery, a preparation method thereof and an electrical device, wherein the solid electrolyte comprises a porous support membrane and a solid electrolyte body at least arranged in the pore structure of the porous support membrane, an inorganic filler and a coupling agent, wherein the solid electrolyte body comprises a polymer and an electrolyte salt, the mass of the coupling agent is 0.01% to 10% of the mass of the solid electrolyte body, and the porosity of the porous support membrane is greater than or equal to 70%. By regulating the composition and structure of the solid electrolyte, adjusting its ion transfer rate and mechanical strength within a reasonable range, and improving the toughness of the solid electrolyte, achieving close contact between the solid electrolyte and the electrode, and reducing the interface resistance of the secondary battery during the charge and discharge process, the electrochemical performance of the secondary battery containing the solid electrolyte, such as cycle stability and high voltage resistance, is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a solid electrolyte, a secondary battery, a preparation method thereof, and an electrical device. Background Art

[0002] In the context of global energy structure transformation and growing demand for mobile energy, solid-state batteries have become the forefront of battery technology research with their high energy density and excellent safety. The performance of solid-state batteries mainly depends on solid electrolytes, a key material that not only affects the ion conduction efficiency, but is also directly related to the mechanical stability and interface compatibility of the battery.

[0003] CN113363561A discloses a high-strength solid electrolyte membrane, which includes a porous support membrane and a solid electrolyte present on both sides and in the pores of the porous support membrane, wherein the solid electrolyte includes a polymer electrolyte, an inorganic solid electrolyte and a lithium salt; the porous support membrane is used to fill part of the solid electrolyte in the pores of the carrier, thereby improving the bonding strength between the support membrane and the solid electrolyte and the mechanical strength of the electrolyte membrane, and simultaneously improving the room temperature ionic conductivity of the electrolyte membrane; the polymer solid electrolyte and the inorganic solid electrolyte are used as a composite electrolyte to improve the mechanical strength of the electrolyte membrane and its contact with the electrode. However, the bonding force and compatibility between the porous support membrane and the electrolyte, and between the polymer solid electrolyte and the inorganic solid electrolyte in the solid electrolyte membrane are still insufficient, which affects the structural stability of the solid electrolyte membrane, and the contact between the solid electrolyte membrane and the electrode is not enough, and the electrode / solid electrolyte interface problem has not been substantially solved, resulting in the electrochemical performance of the secondary battery being limited. Summary of the invention

[0004] The present application provides a solid electrolyte, a secondary battery, a preparation method thereof, and an electrical device to improve the electrochemical performance of a secondary battery containing a solid electrolyte.

[0005] In a first aspect of the present application, a solid electrolyte is provided, comprising a porous support membrane and a solid electrolyte body, an inorganic filler and a coupling agent arranged at least in the pore structure of the porous support membrane, wherein the solid electrolyte body contains a polymer and an electrolyte salt, the mass of the coupling agent is 0.01% to 10% of the mass of the solid electrolyte body, and the porosity of the porous support membrane is greater than or equal to 70%.

[0006] In some embodiments, the porosity of the porous support membrane is 70% to 99%.

[0007] In some embodiments, the porous support membrane has a thickness of 1 μm to 200 μm.

[0008] In some embodiments, the mass of the inorganic filler is 0.05% to 50% of the total mass of the solid electrolyte body, the inorganic filler and the coupling agent.

[0009] In some embodiments, the solid electrolyte body further comprises at least one of an initiator, a catalyst and an additive.

[0010] In some embodiments, the inorganic filler includes at least one of an inorganic solid electrolyte material, an inorganic oxide, a silicate mineral material, and a composite material thereof.

[0011] In some embodiments, the average particle size D50 of the inorganic filler is 0.01 μm to 50 μm.

[0012] In some embodiments, the coupling agent includes at least one of a silane coupling agent, a titanate coupling agent, an aluminate coupling agent, an aluminum zirconate coupling agent, and an organic complex.

[0013] In some embodiments, the electrolyte salt includes at least one of a lithium-containing inorganic salt, a lithium-containing organic salt, a sodium-containing inorganic salt, a sodium-containing organic salt, and a multi-salt complex.

[0014] In some embodiments, the polymerized monomer of the polymer includes at least one of a monomer containing an unsaturated bond and a monomer having a cyclic structure.

[0015] In some embodiments, the porous support membrane includes at least one of a porous organic insulating film and a porous inorganic insulating film, the material of the porous organic insulating film includes at least one of cellulose fiber, polypropylene fiber, polyethylene fiber, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyvinylidene fluoride-acrylonitrile copolymer, polyether sulfone, polyacrylonitrile, polyvinylidene chloride, polyimide, polyurethane, polyvinyl chloride, polyvinyl carbonate and polypropylene carbonate, and the material of the porous inorganic insulating film includes at least one of glass fiber, boron fiber, ceramic fiber, silica, aluminum oxide and titanium dioxide.

[0016] In some embodiments, the inorganic solid electrolyte material includes at least one of an oxide solid electrolyte, a sulfide solid electrolyte, a halide solid electrolyte, an oxysulfide solid electrolyte, an oxyhalide solid electrolyte, and a composite solid electrolyte thereof.

[0017] In some embodiments, the inorganic oxide includes at least one of silicon dioxide, titanium dioxide, and aluminum oxide.

[0018] In some embodiments, the silicate mineral material includes at least one of rectorite, montmorillonite, kaolin, mica powder, talc, attapulgite, halloysite, sepiolite, vermiculite, and wollastonite.

[0019] In some embodiments, the initiator includes at least one of an azo initiator, an organic peroxide initiator, an inorganic peroxide initiator, a redox initiator, and an ionic initiator.

[0020] In some embodiments, the catalyst includes at least one of a Lewis acid catalyst, a cationic catalyst, an anionic catalyst, a coordination catalyst, and a rare earth metal catalyst.

[0021] In some embodiments, the additive includes at least one of fluoroethylene carbonate, succinonitrile, polyethylene glycol, and polyethylene glycol dimethyl ether.

[0022] A second aspect of the present application provides a method for preparing a solid electrolyte, comprising the following steps:

[0023] A porous support membrane is placed in a mixed slurry comprising a precursor solution, an inorganic filler and a coupling agent, and solidified so that the inorganic filler, the coupling agent and the solid electrolyte body are at least arranged in the pore structure of the porous support membrane to obtain the solid electrolyte; the precursor solution comprises a polymerized monomer and an electrolyte salt, the solid electrolyte body comprises a polymer formed by the polymerized monomer and the electrolyte salt, the mass of the coupling agent is 0.01% to 10% of the mass of the solid electrolyte body, and the porosity of the porous support membrane is greater than or equal to 70%.

[0024] The third aspect of the present application provides a secondary battery, comprising a positive electrode plate, a negative electrode plate, and at least one of the solid electrolyte described in the first aspect of the present application and the solid electrolyte prepared by the preparation method described in the second aspect of the present application.

[0025] In a fourth aspect of the present application, a method for preparing a secondary battery is provided, comprising the following steps:

[0026] Providing a semi-finished battery product including a positive electrode sheet, a negative electrode sheet and a porous support membrane, wherein the porous support membrane is arranged between the positive electrode sheet and the negative electrode sheet, and the porosity of the porous support membrane is greater than or equal to 70%;

[0027] A mixed slurry containing a precursor solution, an inorganic filler and a coupling agent is injected into the battery semi-finished product and solidified so that the inorganic filler, the coupling agent and the solid electrolyte body are at least arranged in the pore structure of the porous support membrane to obtain the secondary battery containing a solid electrolyte; the precursor solution contains a polymerized monomer and an electrolyte salt, the solid electrolyte body contains a polymer formed by the polymerized monomer and the electrolyte salt, and the mass of the coupling agent is 0.01% to 10% of the mass of the solid electrolyte body.

[0028] In some embodiments, the solid-liquid interface contact angle between the precursor solution and the porous support membrane in the secondary battery is 0-50°.

[0029] In some embodiments, the curing process conditions include: a curing temperature of 25° C. to 100° C., and a curing time of 0.5 h to 300 h.

[0030] In some embodiments, the inorganic filler accounts for 0.05% to 50% by mass in the mixed slurry.

[0031] In some embodiments, the coupling agent accounts for 0.01% to 10% by mass in the precursor solution.

[0032] In a fifth aspect of the present application, there is provided an electrical device comprising at least one of the secondary battery described in the third aspect of the present application and the secondary battery prepared by the preparation method described in the fourth aspect of the present application.

[0033] Compared with traditional technologies, the above solid electrolytes have at least the following advantages:

[0034] Controlling the porosity of the porous support film in the above-mentioned solid electrolyte within a reasonable range can provide a large number of ion transmission channels and mechanical support, the electrolyte salt can improve the ion migration rate and ion conductivity of the solid electrolyte, the polymer can enhance the mechanical strength and flexibility of the solid electrolyte, the addition of inorganic fillers can not only improve the ion conductivity of the solid electrolyte, but also enhance its mechanical strength and high-voltage resistance, the use of coupling agents can improve the dispersibility of inorganic fillers, significantly improve the interface bonding force and compatibility between inorganic fillers and polymers, thereby improving the interface bonding force between the porous support film, the solid electrolyte body and the inorganic filler, and enhancing the structural stability and ion transmission rate of the solid electrolyte. Therefore, by regulating the composition and structure of the solid electrolyte, adjusting its ion transmission rate and mechanical strength within a reasonable range, while improving the toughness of the solid electrolyte, achieving close contact between the solid electrolyte and the electrode, and reducing the interface resistance of the secondary battery during the charge and discharge process, the electrochemical properties of the secondary battery containing the solid electrolyte, such as cycle stability and high-voltage resistance, are improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 The surface and cross-sectional SEM photos and contact angle projection diagram of the polypropylene fiber porous support membrane used in Example 1 of the present application; Figure 1 a in the figure is the surface SEM photo of the polypropylene fiber porous support membrane. Figure 1 b is a cross-sectional SEM photo of the polypropylene fiber porous support membrane. Figure 1 The c in the figure is the contact angle projection diagram.

[0036] Figure 2 The surface and cross-sectional SEM photos of the solid electrolyte in Example 1 of the present application and the corresponding EDS element distribution map; Figure 2 a in the figure is the surface SEM photo of the solid electrolyte and the corresponding EDS element distribution map. Figure 2 b in the figure is a cross-sectional SEM photograph of the solid electrolyte and the corresponding EDS element distribution map.

[0037] Figure 3 It is the ionic conductivity of the solid electrolyte in Example 1 and Comparative Example 1 of the present application at 25°C.

[0038] Figure 4 The surface and cross-sectional SEM photos and contact angle projection diagrams of the uniaxially stretched polypropylene film used in Comparative Example 1 of the present application; Figure 4 a in the figure is the surface SEM photo of uniaxially stretched polypropylene film. Figure 4 b is a cross-sectional SEM photo of a uniaxially stretched polypropylene film. Figure 4 The c in the figure is the contact angle projection diagram.

[0039] Figure 5 The surface and cross-sectional SEM photos of the solid electrolyte in Comparative Example 1 of the present application and the corresponding EDS element distribution map; Figure 5 a in the figure is the surface SEM photo of the solid electrolyte and the corresponding EDS element distribution map. Figure 5 b in the figure is a cross-sectional SEM photograph of the solid electrolyte and the corresponding EDS element distribution map.

[0040] Figure 6 The surface SEM photo and contact angle projection diagram of the cellulose fiber porous support membrane used in Example 2 of the present application; Figure 6 a in the figure is the surface SEM photo of the cellulose fiber porous support membrane. Figure 6 b in the figure is the contact angle projection diagram.

[0041] Figure 7 The surface and cross-sectional SEM photos of the solid electrolyte in Example 2 of the present application; Figure 7 a in the figure is the surface SEM photo of the solid electrolyte. Figure 7 b in FIG. is a cross-sectional SEM photograph of the solid electrolyte.

[0042] Figure 8 It is the ionic conductivity of the solid electrolyte in Example 2, Comparative Example 2 and Comparative Example 3 of the present application at 25°C.

[0043] Fig. 9 The cycle performance of the solid-state batteries prepared in Example 2 and Comparative Example 2 of the present application.

[0044] Fig.10The surface SEM photo and contact angle projection diagram of the glass fiber porous support membrane used in Example 3 of the present application; Fig.10 a in the figure is the surface SEM photo of the glass fiber porous support membrane. Fig.10 b in the figure is the contact angle projection diagram.

[0045] Fig.11 The surface and cross-sectional SEM photos of the solid electrolyte in Example 3 of the present application and the corresponding EDS element distribution map; Fig.11 a in the figure is the surface SEM photo of the solid electrolyte and the corresponding EDS element distribution map. Fig.11 b in the figure is a cross-sectional SEM photograph of the solid electrolyte and the corresponding EDS element distribution map.

[0046] Fig.12 This is the charge and discharge curve of the solid-state battery prepared in Example 3 of the present application.

[0047] Fig.13 The surface SEM photo and contact angle projection diagram of the polyvinylidene fluoride porous support membrane used in Example 5 of the present application; Fig.13 a in the figure is the surface SEM photo of the porous support membrane of polyvinylidene fluoride. Fig.13 b in the figure is the contact angle projection diagram.

[0048] Fig.14 Surface SEM photograph of the solid electrolyte in Example 5 of the present application and the corresponding EDS element distribution map.

[0049] Fig.15 This is the charge and discharge curve of the solid-state battery prepared in Example 5 of the present application. DETAILED DESCRIPTION

[0050] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.

[0051] In this application, "first aspect", "second aspect", "third aspect", etc. are used only for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.

[0052] In this application, "optionally", "optional", and "optional" mean optional or dispensable, that is, any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.

[0053] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0054] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0055] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as those commonly understood by technicians in the technical field of this application. The terms used in this application and in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used in this application includes any and all combinations of one or more related listed items. The term "multiple" in this application means at least two, such as two, three, etc., unless otherwise clearly and specifically limited.

[0056] In one embodiment of the present application, a solid electrolyte is provided, which includes a porous support membrane and a solid electrolyte body, an inorganic filler and a coupling agent arranged at least in the pore structure of the porous support membrane, wherein the solid electrolyte body contains a polymer and an electrolyte salt, the mass of the coupling agent is 0.01% to 10% of the mass of the solid electrolyte body, and the porosity of the porous support membrane is greater than or equal to 70%.

[0057] The porosity of the porous support membrane is controlled within the above range, which can provide a large number of ion transmission channels and mechanical support. The electrolyte salt can improve the ion migration rate and ion conductivity of the solid electrolyte. The polymer can enhance the mechanical strength and flexibility of the solid electrolyte. The addition of inorganic fillers can not only improve the ion conductivity of the solid electrolyte, but also enhance its mechanical strength and high-voltage resistance. The use of coupling agents can improve the dispersibility of inorganic fillers, significantly improve the interface bonding force and compatibility between inorganic fillers and polymers, thereby improving the interface bonding force between the porous support membrane, the solid electrolyte body and the inorganic filler, and enhancing the structural stability and ion transmission rate of the solid electrolyte. Therefore, by regulating the composition and structure of the solid electrolyte, adjusting its ion transmission rate and mechanical strength within a reasonable range, and improving the toughness of the solid electrolyte, achieving close contact between the solid electrolyte and the electrode, and reducing the interface resistance of the secondary battery during the charge and discharge process, the mechanical stability and electrochemical properties of the secondary battery containing the solid electrolyte, such as cycle stability and high-voltage resistance, are improved.

[0058] Since the solid electrolyte can work stably at high voltage, the energy density of the secondary battery can be improved. In addition, the solid electrolyte does not contain flammable organic solvents, so the safety performance of the secondary battery can be significantly improved and the safety risks during use can be reduced.

[0059] It can be understood that the mass of the coupling agent can be, for example, 0.01%, 2%, 4%, 6%, 8%, 10% of the mass of the solid electrolyte body, or a range between any two of the foregoing, and the porosity of the porous support membrane includes but is not limited to: 70%, 73%, 76%, 80%, 83%, 86%, 90%, 93%, 96%, 99%.

[0060] In some embodiments, the porosity of the porous support membrane is 70% to 99%. Controlling the porosity of the porous support membrane within the above range is beneficial to further improve the ionic conductivity of the solid electrolyte.

[0061] In some embodiments, the thickness of the porous support membrane is 1 μm to 200 μm. Such a design can further improve the mechanical strength and flexibility of the solid electrolyte. It is understood that the thickness of the porous support membrane includes but is not limited to: 1 μm, 10 μm, 30 μm, 50 μm, 70 μm, 100 μm, 120 μm, 150 μm, 180 μm, 200 μm.

[0062] In some embodiments, the mass of the inorganic filler is 0.05% to 50% of the total mass of the solid electrolyte body, the inorganic filler and the coupling agent. Controlling the mass of the inorganic filler to the above range is conducive to further improving the ionic conductivity, mechanical strength and high voltage resistance of the solid electrolyte. Optionally, the above percentages include but are not limited to: 0.05%, 2%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%. Further, the mass of the inorganic filler is 5% to 20% of the total mass of the solid electrolyte body, the inorganic filler and the coupling agent.

[0063] In some embodiments, the mass of the coupling agent is 0.01% to 5% of the mass of the solid electrolyte body. Such a design can further regulate the ion transfer rate and mechanical strength of the solid electrolyte, further reduce the interface resistance of the secondary battery during the charge and discharge process, and further improve the mechanical stability and electrochemical performance of the secondary battery containing the solid electrolyte.

[0064] In some embodiments, the solid electrolyte body further comprises at least one of an initiator, a catalyst and an additive.

[0065] In some embodiments, the initiator includes at least one of an azo initiator, an organic peroxide initiator, an inorganic peroxide initiator, a redox initiator, and an ionic initiator. Thus, the polymerization reaction can be carried out efficiently. Optionally, the azo initiator includes but is not limited to azobisisobutyronitrile (AIBN). Optionally, the organic peroxide initiator includes but is not limited to dibenzoyl peroxide (BPO).

[0066] In some embodiments, the catalyst includes at least one of a Lewis acid catalyst, a cationic catalyst, an anionic catalyst, a coordination catalyst, and a rare earth metal catalyst.

[0067] In some embodiments, the additive includes at least one of fluoroethylene carbonate, succinonitrile, polyethylene glycol and polyethylene glycol dimethyl ether.

[0068] In some embodiments, the inorganic filler includes at least one of an inorganic solid electrolyte material, an inorganic oxide, a silicate mineral material, and a composite material thereof. The composite material includes, but is not limited to, a composite material comprising an inorganic solid electrolyte material, a composite material comprising an inorganic oxide, a composite material comprising a silicate mineral material, and at least one of a composite material formed of an inorganic solid electrolyte material and / or an inorganic oxide and / or a silicate mineral material.

[0069] In some embodiments, the inorganic solid electrolyte material includes at least one of an oxide solid electrolyte, a sulfide solid electrolyte, a halide solid electrolyte, an oxysulfide solid electrolyte, an oxyhalide solid electrolyte, and a composite solid electrolyte thereof.

[0070] In some embodiments, the inorganic oxide includes at least one of silicon dioxide, titanium dioxide, and aluminum oxide.

[0071] In some embodiments, the silicate mineral material includes at least one of rectorite, montmorillonite, kaolin, mica powder, talc, attapulgite, halloysite, sepiolite, vermiculite and wollastonite.

[0072] In some embodiments, the average particle size D50 of the inorganic filler is 0.01 μm to 50 μm. It is understood that the average particle size D50 of the inorganic filler includes but is not limited to: 0.01 μm, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm.

[0073] In some embodiments, the coupling agent includes at least one of a silane coupling agent, a titanate coupling agent, an aluminate coupling agent, an aluminum zirconate coupling agent, and an organic complex. The use of the above-mentioned types of coupling agents can further enhance the interfacial bonding force between the porous support membrane, the solid electrolyte body, and the inorganic filler, which is beneficial to further enhance the electrochemical performance of the secondary battery. Optionally, the silane coupling agent includes but is not limited to γ-methacryloxypropyltrimethoxysilane (KH570).

[0074] In some embodiments, the electrolyte salt includes at least one of a lithium-containing inorganic salt, a lithium-containing organic salt, a sodium-containing inorganic salt, a sodium-containing organic salt, and a multi-salt complex.

[0075] In some embodiments, the lithium-containing organic salt includes lithium bistrifluoromethanesulfonyl imide (LiTFSI), and the sodium-containing organic salt includes sodium bistrifluoromethanesulfonyl imide (NaTFSI).

[0076] In some embodiments, the lithium-containing inorganic salt includes at least one of lithium hexafluorophosphate (LiPF6) and lithium perchlorate (LiClO4), and the sodium-containing inorganic salt includes at least one of sodium hexafluorophosphate (NaPF6) and lithium perchlorate (NaClO4).

[0077] In some embodiments, the electrolyte salt includes at least one of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and sodium bis(trifluoromethanesulfonyl)imide (NaTFSI). Thus, the ion mobility of the solid electrolyte can be further enhanced.

[0078] In some embodiments, the polymerized monomer of the polymer includes at least one of a monomer including an unsaturated bond and a monomer having a cyclic structure.

[0079] In some embodiments, the polymer monomer includes at least one of ethylene glycol dimethacrylate (PEGDA), vinyl ethylene carbonate (VEC) and 1,3-dioxolane (DOL). Thus, the ionic conductivity and mechanical strength of the solid electrolyte can be further improved, which is more conducive to improving the cycle stability of the secondary battery.

[0080] In some embodiments, the porous support membrane includes at least one of a porous organic insulating thin film and a porous inorganic insulating thin film.

[0081] In some embodiments, the material of the porous organic insulating film includes at least one of cellulose fiber, polypropylene fiber, polyethylene fiber, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyvinylidene fluoride-acrylonitrile copolymer, polyether sulfone, polyacrylonitrile, polyvinylidene chloride, polyimide, polyurethane, polyvinyl chloride, polyvinyl carbonate and polypropylene carbonate.

[0082] In some embodiments, the cellulose fibers include paper-based fibers, and the paper-based fibers include at least one of rice paper, rough paper, copy paper, and filter paper.

[0083] In some embodiments, the material of the porous inorganic insulating film includes at least one of glass fiber, boron fiber, ceramic fiber, silicon dioxide, aluminum oxide and titanium dioxide.

[0084] In some embodiments, the material of the porous support membrane includes at least one of polypropylene fiber, cellulose fiber, glass fiber and polyvinylidene fluoride. The porous support membrane of the above-mentioned materials has a rich pore structure and excellent mechanical properties and chemical stability.

[0085] Another embodiment of the present application provides a method for preparing a solid electrolyte, characterized in that it includes the following steps:

[0086] The porous support membrane is placed in a mixed slurry containing a precursor solution, an inorganic filler and a coupling agent, and solidified so that the inorganic filler, the coupling agent and the solid electrolyte body are at least arranged in the pore structure of the porous support membrane to obtain a solid electrolyte; the precursor solution contains a polymerized monomer and an electrolyte salt, the solid electrolyte body contains a polymer formed by the polymerized monomer and an electrolyte salt, the mass of the coupling agent is 0.01% to 10% of the mass of the solid electrolyte body, and the porosity of the porous support membrane is greater than or equal to 70%.

[0087] The above preparation method is relatively simple and can reduce the preparation cost of solid electrolytes. By regulating the composition and structure of the solid electrolyte prepared by the above preparation method, the ion transfer rate and mechanical strength thereof are adjusted within a reasonable range, the toughness of the solid electrolyte is improved, and close contact between the solid electrolyte and the electrode is achieved, and the interface resistance of the secondary battery during the charge and discharge process is reduced, thereby improving the mechanical stability and electrochemical performance of the secondary battery containing the solid electrolyte, such as cycle stability and high voltage resistance.

[0088] Since the solid electrolyte can work stably at high voltage, the energy density of the secondary battery can be improved. In addition, the solid electrolyte does not contain flammable organic solvents, so the safety performance of the secondary battery can be significantly improved and the safety risks during use can be reduced.

[0089] It can be understood that the solid electrolyte body is formed from a precursor solution.

[0090] In some embodiments, the porosity of the porous support membrane is 70% to 99%. Controlling the porosity of the porous support membrane within the above range is beneficial to further improve the ionic conductivity of the solid electrolyte.

[0091] In some embodiments, the solid-liquid interface contact angle between the precursor solution and the porous support membrane is 0 to 50°. By controlling the solid-liquid interface contact angle between the porous support membrane and the precursor solution, the interfacial compatibility between the solid electrolyte and the electrode can be optimized, thereby further improving the interfacial stability and the overall performance of the secondary battery. The above contact angles include, but are not limited to: 0, 5°, 10°, 15°, 20°, 25°, 30°, 35°, 40°, 45°, 50°.

[0092] In some embodiments, the curing process conditions include: the curing temperature is 25°C to 100°C, and the curing time is 0.5h to 300h. Thus, the polymerization reaction can be fully carried out. Further, the curing process conditions include: the curing temperature is 80°C, and the curing time is 0.5h to 12h.

[0093] In some embodiments, the mass proportion of the inorganic filler in the mixed slurry is 0.05% to 50%. The above mass proportion includes but is not limited to: 0.05%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%.

[0094] In some embodiments, the mass proportion of the coupling agent in the precursor solution is 0.01% to 10%.

[0095] In some embodiments, the precursor solution further comprises at least one of an initiator, a catalyst and an additive.

[0096] In some embodiments, the initiator includes at least one of an azo initiator, an organic peroxide initiator, an inorganic peroxide initiator, a redox initiator, and an ionic initiator. Thus, the polymerization reaction can be carried out efficiently. Optionally, the azo initiator includes but is not limited to azobisisobutyronitrile (AIBN). Optionally, the organic peroxide initiator includes but is not limited to dibenzoyl peroxide (BPO).

[0097] In some embodiments, the catalyst includes at least one of a Lewis acid catalyst, a cationic catalyst, an anionic catalyst, a coordination catalyst, and a rare earth metal catalyst.

[0098] In some embodiments, the additive includes at least one of fluoroethylene carbonate, succinonitrile, polyethylene glycol and polyethylene glycol dimethyl ether.

[0099] By controlling the process conditions of the above-mentioned preparation method, a solid electrolyte in one embodiment of the present application can be obtained.

[0100] Another embodiment of the present application provides a secondary battery, including a positive electrode sheet, a negative electrode sheet, and at least one of the above-mentioned solid electrolyte of the present application and the solid electrolyte prepared by the above-mentioned preparation method of the present application. The above-mentioned secondary battery includes but is not limited to at least one of a solid-state lithium ion battery, a solid-state sodium ion battery, a solid-state lithium metal battery, and a solid-state sodium metal battery. It is understood that the positive electrode sheet contains a positive electrode active material, the negative electrode sheet contains a negative electrode active material, and the positive electrode sheet and the negative electrode sheet can be prepared by a preparation method commonly used in the art.

[0101] Another embodiment of the present application also provides a method for preparing a secondary battery, comprising the following steps:

[0102] Providing a semi-finished battery product including a positive electrode sheet, a negative electrode sheet and a porous support membrane, wherein the porous support membrane is arranged between the positive electrode sheet and the negative electrode sheet, and the porosity of the porous support membrane is greater than or equal to 70%;

[0103] A mixed slurry containing a precursor solution, an inorganic filler and a coupling agent is injected into a semi-finished battery product and solidified so that the inorganic filler, the coupling agent and the solid electrolyte body are at least arranged in the pore structure of the porous support membrane to obtain a secondary battery containing a solid electrolyte; the precursor solution contains a polymerized monomer and an electrolyte salt, the solid electrolyte body contains a polymer formed by the polymerized monomer and an electrolyte salt, and the mass of the coupling agent is 0.01% to 10% of the mass of the solid electrolyte body.

[0104] The above preparation method is relatively simple and can reduce the preparation cost of secondary batteries. By regulating the composition and structure of the solid electrolyte of the secondary battery prepared by the above preparation method, the ion transfer rate and mechanical strength thereof are adjusted within a reasonable range, the toughness of the solid electrolyte is improved, the close contact between the solid electrolyte and the electrode is achieved, and the interface resistance of the secondary battery during the charge and discharge process is reduced, thereby improving the mechanical stability and electrochemical performance of the secondary battery containing the solid electrolyte, such as cycle stability and high voltage resistance.

[0105] The polymer, electrolyte salt, coupling agent and inorganic filler in the above preparation method are used in combination and in situ polymerization technology is adopted to further improve the ion migration rate of the solid electrolyte in the secondary battery, enhance its ion conductivity, improve the interface bonding force between the solid electrolyte and the electrode, further reduce the interface resistance of the battery during the charge and discharge process, thereby further improving the electrochemical performance of the secondary battery.

[0106] Since the solid electrolyte can work stably at high voltage, the energy density of the secondary battery can be improved. In addition, the solid electrolyte does not contain flammable organic solvents, so the safety performance of the secondary battery can be significantly improved and the safety risks during use can be reduced.

[0107] The solid electrolyte in the secondary battery can be prepared by in-situ thermal polymerization of a high-porosity porous support membrane composite in-situ polymerization of a precursor solution and a mixed slurry of an inorganic filler and a coupling agent.

[0108] Coupling agents play an important role in solid electrolytes. First, coupling agents can significantly improve the interfacial compatibility of organic and inorganic components when preparing mixed slurries, so that inorganic fillers can be evenly dispersed in the precursor solution for a long time; secondly, during the polymerization process, the organic-philic end functional groups of the coupling agent can undergo graft polymerization reactions with the polymerized monomers, that is, the coupling agent can act as a bridge between the solid electrolyte body and the inorganic filler, effectively enhancing the interfacial bonding force between the two, which is beneficial to improving the structural stability and ion transfer rate of the solid electrolyte.

[0109] In some embodiments, the solid-liquid interface contact angle between the precursor solution and the porous support membrane in the secondary battery is 0 to 50°. By controlling the solid-liquid interface contact angle between the porous support membrane and the precursor solution, the interface compatibility between the solid electrolyte and the electrode can be optimized, thereby further improving the interface stability and the overall performance of the secondary battery.

[0110] In some embodiments, the curing process conditions include: the curing temperature is 25°C to 100°C, and the curing time is 0.5h to 300h. Thus, the polymerization reaction can be fully carried out. Further, the curing process conditions include: the curing temperature is 80°C, and the curing time is 0.5h to 12h.

[0111] In some embodiments, the mass proportion of the inorganic filler in the mixed slurry is 0.05% to 50%.

[0112] In some embodiments, the mass proportion of the coupling agent in the precursor solution is 0.01% to 10%.

[0113] In some embodiments, the precursor solution further comprises at least one of an initiator, a catalyst and an additive.

[0114] By controlling the process conditions of the above preparation method, a secondary battery in another embodiment of the present application can be obtained.

[0115] The present application also provides an electric device, comprising at least one of the secondary battery mentioned above and the secondary battery prepared by the preparation method mentioned above. The electric device includes but is not limited to at least one of an electric car, a laptop computer, a mobile phone and an energy storage device.

[0116] The solid electrolyte and its preparation method, secondary battery and its preparation method provided in this application can not only improve the comprehensive performance of solid-state batteries, but also promote the commercialization process of solid-state battery technology, and provide safer and more efficient energy solutions for portable electronic devices, electric vehicles and large-scale energy storage systems.

[0117] In order to further illustrate the present application, the technical scheme of the present application is described in detail below in conjunction with specific examples. If no specific technology or conditions are specified in the examples, the technology or conditions described in the literature in the field or the product instructions are used. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.

[0118] Example 1

[0119] The solid electrolyte and solid-state battery are prepared as follows:

[0120] (1) Selection and preparation of porous support membrane: A porous organic insulating film made of polypropylene fiber was selected as the porous support membrane. The porosity of the membrane was 83% and the thickness was 100 μm.

[0121] (2) Preparation of in-situ polymerization precursor solution: Ethylene glycol dimethacrylate (PEGDA) was used as the polymerization monomer, lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) was used as the electrolyte salt, and fluoroethylene carbonate (FEC) was used as the additive. They were mixed in a mass ratio of 45:30:25, and 0.15% of azobisisobutyronitrile (AIBN) by mass of PEGDA was added as an initiator. Under argon protection, these components were fully mixed at room temperature.

[0122] (3) Preparation of mixed slurry: mica powder (D50 is 2.6 μm) is selected as the inactive inorganic filler, and its mass proportion is 5% of the total mass of the mixed slurry; γ-methacryloxypropyltrimethoxysilane (KH570 silane coupling agent) is selected as the coupling agent, and its mass proportion is 0.05% of the total mass of the in-situ polymerization precursor solution; at room temperature, the in-situ polymerization precursor solution is fully mixed with the mica powder inorganic filler and KH570 silane coupling agent to form a uniform mixed slurry.

[0123] (4) In-situ solidification process: In an argon atmosphere with a water and oxygen value of ≤0.1 ppm, the -2 The prepared mixed slurry is injected into a battery semi-finished product equipped with a polypropylene fiber porous support membrane, a positive electrode sheet and a negative electrode sheet (the porous support membrane is located between the positive electrode sheet and the negative electrode sheet) with a filling amount (based on the area of ​​the porous support membrane), and reacted at 80°C for 1 hour to obtain a solid electrolyte and a solid-state battery (lithium-ion secondary battery).

[0124] The polypropylene fiber porous support membrane used in Example 1 has a porosity of up to 83%. Its surface SEM photograph is as follows: Figure 1 As shown in a in the figure, it can be seen that the support membrane is made of polypropylene fibers with a diameter of 1μm~3μm, with a large number of micron-sized pores. The cross-sectional SEM photo (such as Figure 1 (b) also shows a rich pore structure. This porous structure is conducive to accommodating more mixed slurries composed of in-situ polymerization precursor solution, inorganic fillers and coupling agents, forming a solid electrolyte with uniform components, and providing a large number of ion transmission channels. In addition, the initial contact angle (0 seconds) between the polypropylene fiber porous support membrane and the in-situ polymerization precursor solution is 124.8°, which decreases to 38.2° after 60 seconds (as shown in Fig. Figure 1 (c) shows that the polypropylene fiber porous support membrane has good wetting properties, which is an important factor in preparing solid electrolytes with good composite morphology, fine interface structure and low interface impedance.

[0125] Surface and cross-sectional SEM images of the solid electrolyte prepared in Example 1 ( Figure 2Figures a and b) show that the pores of the polypropylene fiber porous support membrane have been filled with the in-situ cured mixed slurry, and the micron-sized inorganic filler (mica powder) has also been well embedded in it.

[0126] Figure 2 Figures a and b also show the surface and cross-sectional EDS element distribution of the solid electrolyte prepared in Example 1. Among them, the C element mainly comes from the porous support membrane of polypropylene fibers, and part of it comes from PEGDA, LiTFSI and KH570. Its distribution mainly reflects the outline of the porous support membrane of polypropylene fibers; the O element comes from PEGDA, LiTFSI, mica powder and KH570, and its distribution reflects the overall morphology of the solid electrolyte body (i.e., PEGDA and LiTFSI) and the inorganic filler; the F and S elements only come from LiTFSI, and their distribution reflects the dispersion state of LiTFSI in the solid electrolyte; the Si element mainly comes from mica powder, and a very small part comes from KH570, and its distribution reflects the position information of the inorganic filler in the solid electrolyte. The C element shows complementary and uniform distribution characteristics with the O, F, and S elements, indicating that the porous support membrane of polypropylene fibers and the solid electrolyte body belong to the "interpenetrating" deep composite morphology. The Si element is evenly distributed on the surface and cross-section, indicating that the mica powder is distributed in a three-dimensional manner deep inside the solid electrolyte, rather than a flat distribution floating on the surface. The pore structure of the polypropylene fiber porous support membrane is filled with the solid electrolyte body, inorganic filler and coupling agent.

[0127] Depend on Figure 3 It can be seen that the room temperature ionic conductivity of the solid electrolyte prepared in Example 1 is (1.18±0.02)×10 -4 S cm -1 , showing good ion transport properties. It is worth mentioning that the coefficient of dispersion of this value is only 1.7%, indicating that the solid electrolyte material prepared under the same preparation process has a high batch consistency.

[0128] Comparative Example 1

[0129] The preparation of the solid electrolyte and the solid-state battery in this comparative example is basically the same as that in Example 1, except that the support membrane used is a uniaxially stretched polypropylene film having a porosity of 53% and a thickness of 25 μm.

[0130] Figure 4a and b in the figure show that the uniaxially stretched polypropylene film of comparative example 1 has a large number of submicron-sized pores in a narrow and long elliptical structure, but these pores are much smaller than those of the polypropylene fiber porous support membrane in Example 1, which not only cannot accommodate enough mixed slurry composed of in-situ polymerization precursor solution, inorganic filler and coupling agent, but also cannot allow inorganic fillers with micron size to enter therein.

[0131] In addition, by Figure 4 As can be seen from c, the contact angle of the unidirectional polypropylene film of Comparative Example 1 is as high as 65.5° (after contacting the in-situ polymerization precursor solution for 60 seconds), indicating that it has poor wetting properties and the in-situ polymerization precursor solution is difficult to penetrate into it. Figure 5 The SEM photos and EDS element distribution diagrams of the solid electrolyte fully verify this point: the F element is concentrated only on the surface of the solid electrolyte, indicating that the solid electrolyte body (i.e., PEGDA and LiTFSI) is only formed in situ on the surface of the polypropylene film. The same is true for the distribution of the Si element. A large amount of Si elements are observed on the surface of the solid electrolyte, but there is almost no Si element in its cross section. This is because the micron-sized mica powder cannot enter the tiny pores of the polypropylene film. Therefore, the solid electrolyte body and the inorganic filler in the solid electrolyte are typically distributed in a "planar" manner floating on the surface, which is a non-ideal composite form.

[0132] Depend on Figure 3 It can be seen that the room temperature ionic conductivity of the solid electrolyte of Comparative Example 1 is only (8.79±5.07)×10 -6 S cm -1 , which is 92.6% lower than that of Example 1. And the coefficient of dispersion of this value is as high as 57.7%, indicating that this solid electrolyte material has low batch consistency.

[0133] Example 2

[0134] The solid electrolyte and solid-state battery are prepared as follows:

[0135] (1) Selection and preparation of porous support membrane: A porous organic insulating film made of cellulose fiber was selected as the support membrane. The porosity of the membrane was 93% and the thickness was 30 μm.

[0136] (2) Preparation of in-situ polymerization precursor solution: PEGDA was used as the polymerization monomer, LiTFSI was used as the electrolyte salt, and FEC was used as the additive. They were mixed in a mass ratio of 30:30:40, and AIBN was added as an initiator at a mass ratio of 0.15% of PEGDA. Under the protection of argon, these components were fully mixed at room temperature.

[0137] (3) Preparation of mixed slurry: mica powder (D50 is 2.6 μm) is selected as the inactive inorganic filler, and its mass proportion is 5% of the total mass of the mixed slurry; KH570 silane coupling agent is selected as the coupling agent, and its mass proportion is 0.05% of the total mass of the in-situ polymerization precursor solution; at room temperature, the in-situ polymerization precursor solution, mica powder inorganic filler and KH570 silane coupling agent are fully mixed to form a uniform mixed slurry.

[0138] (4) In-situ solidification process: In an argon atmosphere with a water and oxygen value of ≤0.1 ppm, the -2 The prepared mixed slurry is injected into a battery semi-finished product equipped with a cellulose fiber porous support membrane, a positive electrode sheet and a negative electrode sheet (the porous support membrane is located between the positive electrode sheet and the negative electrode sheet) with a filling amount (based on the area of ​​the porous support membrane), and reacted at 80°C for 1 hour to obtain a solid electrolyte and a solid-state battery (lithium-ion secondary battery).

[0139] The cellulose fiber porous support membrane used in Example 2 has a rich pore structure (porosity up to 93%). From its surface SEM photo ( Figure 6 As can be seen in a), the support membrane is composed of numerous fine cellulose fibers interwoven to form a large number of micron-sized pores. Figure 6 Figure b shows that the contact angle between the cellulose fiber porous support membrane and the in-situ polymerization precursor solution is 5.5° (after 60 seconds), showing excellent wetting properties.

[0140] Figure 7 a and b are the surface and cross-sectional SEM photos of the solid electrolyte prepared in Example 2, respectively. It can be seen from the figure that the cellulose fiber porous support membrane and the solid electrolyte body of Example 2 together form an "interpenetrating" composite form, and the pores of the cellulose fiber porous support membrane are filled with the mixed slurry after in-situ curing, and the inorganic filler (mica powder) is evenly dispersed therein. The pore structure of the cellulose fiber porous support membrane is filled with the solid electrolyte body, inorganic filler and coupling agent.

[0141] from Figure 8 It can be seen that the room temperature ionic conductivity of the solid electrolyte prepared in Example 2 is (3.69±0.72)×10 -4 S cm -1 , showing excellent ion transport properties. With lithium iron phosphate (LiFePO4, LFP) as the positive electrode active material and lithium metal as the negative electrode active material, and with the solid electrolyte prepared in Example 2, the assembled solid-state battery has a high charge / discharge rate of 2.5V~4.0V and 0.1C (1C= 170 mAh g -1 ) showed up to 164.3 mAh g -1The first cycle discharge specific capacity, and the capacity retention rate after 50 cycles is 90.0%.

[0142] Comparative Example 2

[0143] The preparation of the solid electrolyte and the solid-state battery in this comparative example is basically the same as that in Example 2, except that no mica powder inorganic filler and KH570 silane coupling agent are added to the mixed slurry.

[0144] from Figure 8 It can be seen that the room temperature ionic conductivity of the solid electrolyte prepared in Comparative Example 2 is (1.27±0.29)×10 -4 S cm -1 Compared with Example 2, the capacity of the solid-state battery assembled with LFP as the positive electrode active material and lithium metal as the negative electrode active material and the solid electrolyte prepared in Comparative Example 2 is 160.8 mAh g at the first cycle under the conditions of 2.5V~4.0V and 0.1C. -1 However, it failed after 23 cycles, showing unsatisfactory stability performance, which proves that inorganic fillers play an important role in enhancing the long-term stability of solid-state batteries.

[0145] Comparative Example 3

[0146] The preparation of the solid electrolyte and the solid-state battery in this comparative example is basically the same as that in Example 2, except that no KH570 silane coupling agent is added to the mixed slurry.

[0147] from Figure 8 It can be seen that the room temperature ionic conductivity of the solid electrolyte prepared in Comparative Example 3 is (1.36±0.06)×10 -4 S cm -1 , which is 7.1% higher than that of Comparative Example 2, proving again that inorganic fillers help improve the ionic conductivity of such solid electrolytes. However, the room temperature ionic conductivity of Comparative Example 3 is only 36.8% of that of Example 2, which shows that silane coupling agents play an important role in such solid electrolytes. The presence of silane coupling agents can effectively enhance the compatibility and interfacial bonding between the solid electrolyte body and the inorganic filler, thereby greatly improving the ion transfer rate of such solid electrolytes.

[0148] The solid-state battery assembled with LFP as the positive electrode active material and lithium metal as the negative electrode active material and the solid electrolyte prepared in Comparative Example 3 has a first-cycle discharge capacity of 161.5 mAh g under the conditions of 2.5V~4.0V and 0.1C. -1After 50 cycles, the capacity retention rate is 70.1%. The cycle stability of the solid-state battery in Comparative Example 3 is still far behind that in Example 2, which shows that the coupling agent plays an important role in improving the cycle stability of the solid-state battery.

[0149] Example 3

[0150] The solid electrolyte and solid-state battery are prepared as follows:

[0151] (1) Selection and preparation of porous support membrane: A porous inorganic insulating film made of glass fiber was selected as the support membrane. The porosity of the membrane was 96% and the thickness was 180 μm.

[0152] (2) Preparation of in-situ polymerization precursor solution: PEGDA was used as the polymerization monomer, LiTFSI was used as the electrolyte salt, and FEC was used as the additive. They were mixed in a mass ratio of 45:30:25, and 0.15% of AIBN by mass of PEGDA was added as an initiator. Under argon protection, these components were fully mixed at room temperature.

[0153] (3) Preparation of mixed slurry: Aluminum-doped lithium lanthanum zirconium oxide solid electrolyte (Li 6.4 Al 0.24 La3Zr2O 12 , LALZO, D50 is 0.3μm) is an active inorganic filler, and its mass accounts for 5% of the total mass of the mixed slurry; KH570 silane coupling agent is selected as a coupling agent, and its mass accounts for 1% of the total mass of the in-situ polymerization precursor solution; at room temperature, the in-situ polymerization precursor solution is fully mixed with LALZO inorganic filler and KH570 silane coupling agent to form a uniform mixed slurry.

[0154] (4) In-situ solidification process: In an argon atmosphere with a water and oxygen value of ≤0.1 ppm, the -2 The prepared mixed slurry is injected into a battery semi-finished product equipped with a glass fiber porous support membrane, a positive electrode sheet and a negative electrode sheet (the porous support membrane is located between the positive electrode sheet and the negative electrode sheet) with a filling amount (based on the area of ​​the porous support membrane), and reacted at 80°C for 1 hour to obtain a solid electrolyte and a solid-state battery (lithium-ion secondary battery).

[0155] The glass fiber porous support membrane used in Example 3 has a porosity of up to 96%. Fig.10 As shown in a in the figure, it can be seen that the support membrane is made of interwoven glass fibers, forming a large number of micron-sized pores. The contact angle between the glass fiber porous support membrane in Example 3 and the in-situ polymerization precursor solution is 92.8° (at 0 seconds), and it quickly drops to 0° after 5 seconds (as shown in FIG. Fig.10As shown in b in the figure, it indicates that the glass fiber porous support membrane has a good affinity for the in-situ polymerization precursor solution, thus having excellent wetting properties.

[0156] Fig.11 The surface and cross-sectional SEM photos and EDS element distribution diagrams of the solid electrolyte prepared in Example 3 are shown. It can be seen that the pores of the glass fiber porous support membrane have been filled with the in-situ cured mixed slurry, and the submicron-sized inorganic filler (LALZO) can be completely and evenly coated therein, revealing the good "interpenetrating" composite morphology between the glass fiber porous support membrane and the solid electrolyte body.

[0157] from Fig.12 It can be seen that the room temperature ionic conductivity of the solid electrolyte prepared in Example 3 is (1.95±0.10)×10 -4 S cm -1 . With high nickel ternary cathode material LiNi 0.96 Co 0.03 Mn 0.01 O2 (denoted as NCM96) is used as the positive electrode active material, lithium metal is used as the negative electrode active material, and the solid electrolyte is used together. The assembled solid-state battery has a current of 3.0V~4.5V and 0.05C (1C = 210 mAh g -1 ) has 184.3mAh g -1 The discharge capacity ( Fig.12 ), indicating that the solid-state battery has good high-voltage performance.

[0158] Example 4

[0159] The solid electrolyte and solid-state battery are prepared as follows:

[0160] (1) Selection and preparation of porous support membrane: A porous organic insulating film made of cellulose fiber was selected as the support membrane. The porosity of the membrane was 93% and the thickness was 30 μm.

[0161] (2) Preparation of in-situ polymerization precursor solution: PEGDA was used as the polymerization monomer, LiTFSI was used as the electrolyte salt, and FEC was used as the additive. They were mixed in a mass ratio of 45:30:25, and 0.15% of AIBN by mass of PEGDA was added as an initiator. Under argon protection, these components were fully mixed at room temperature.

[0162] (3) Preparation of mixed slurry: LALZO (D50 is 0.3 μm) is selected as the active inorganic filler, and its mass proportion is 5% of the total mass of the mixed slurry; KH570 silane coupling agent is selected as the coupling agent, and its mass proportion is 1% of the total mass of the in-situ polymerization precursor solution; at room temperature, the in-situ polymerization precursor solution is fully mixed with mica powder inorganic filler and KH570 silane coupling agent to form a uniform mixed slurry.

[0163] (4) In-situ solidification process: In an argon atmosphere with a water and oxygen value of ≤0.1 ppm, the -2 The prepared mixed slurry is injected into a battery semi-finished product equipped with a cellulose fiber porous support membrane, a positive electrode sheet and a negative electrode sheet (the porous support membrane is located between the positive electrode sheet and the negative electrode sheet) with a filling amount (based on the area of ​​the porous support membrane), and reacted at 80°C for 1 hour to obtain a solid electrolyte and a solid-state battery (lithium-ion secondary battery).

[0164] The room temperature ionic conductivity of the solid electrolyte prepared in Example 4 is (1.23±0.03)×10 -4 S cm -1 .

[0165] Example 5

[0166] The preparation of the solid electrolyte and the solid-state battery in this embodiment is basically the same as that in Embodiment 4, except that a porous organic insulating film made of polyvinylidene fluoride is selected as the porous support membrane, and the porosity of the membrane is 92% and the thickness is 110 μm.

[0167] from Fig.13 As can be seen from a in the figure, the SEM photo of the polyvinylidene fluoride porous support membrane used in Example 5 shows that it has a large number of irregular pores of micrometer size. The contact angle of the polyvinylidene fluoride porous support membrane with the in-situ polymerization precursor solution is 40.5° (at 0 seconds), which decreases to 0° after 37 seconds ( Fig.13 b) in the figure indicates that the polyvinylidene fluoride porous support membrane has excellent wetting properties.

[0168] SEM photo and EDS element distribution diagram of the solid electrolyte prepared in Example 5 ( Fig.14 ) shows that the pores of the PVDF porous support membrane have been filled with the in-situ cured mixed slurry to form a uniform composite structure.

[0169] The room temperature ionic conductivity of the solid electrolyte prepared in Example 5 is (1.28±0.78)×10 -4 S cm -1The solid-state battery assembled with NCM96 as the positive electrode active material and lithium metal as the negative electrode active material in combination with the solid electrolyte prepared in Example 5 has a current capacity of 3.0V~4.3V and 0.05C (1C = 210 mAh g -1 ) has 157.1 mAh g -1 The discharge capacity ( Fig.15 ).

[0170] Example 6

[0171] The preparation of the solid electrolyte and solid-state battery in this embodiment is basically the same as that in Example 4, with the only difference being that rectorite is selected as an inactive inorganic filler when preparing the mixed slurry, and its mass accounts for 5% of the total mass of the mixed slurry.

[0172] The room temperature ionic conductivity of the solid electrolyte prepared in Example 6 is (1.15±0.05)×10 -4 S cm -1 .

[0173] Example 7

[0174] The preparation of the solid electrolyte and the solid-state battery in this embodiment is basically the same as that in Example 4, with the only difference being that: when preparing the mixed slurry, mica powder (D50 is 2.6 μm) is selected as an inactive inorganic filler, and its mass accounts for 10% of the total mass of the mixed slurry; the mass of the added KH570 silane coupling agent accounts for 10% of the total mass of the in-situ polymerization precursor solution.

[0175] The room temperature ionic conductivity of the solid electrolyte prepared in Example 7 is (8.60±0.71)×10 -5 S cm -1 .

[0176] Example 8

[0177] The solid electrolyte and solid-state battery are prepared as follows:

[0178] (1) Selection and preparation of porous support membrane: A porous inorganic insulating film made of glass fiber was selected as the support membrane. The porosity of the membrane was 96% and the thickness was 180 μm.

[0179] (2) Preparation of in-situ polymerization precursor solution: Vinyl ethylene carbonate (VEC) was used as the polymerization monomer, sodium bis(trifluoromethylsulfonyl)imide (NaTFSI) was used as the electrolyte salt, and succinonitrile (SN) was used as the additive. They were mixed in a mass ratio of 65:25:10, and then 0.15% of dibenzoyl peroxide (BPO) by mass of VEC was added as an initiator. Under the protection of argon, these components were fully mixed at room temperature.

[0180] (3) Preparation of mixed slurry: Titanium dioxide (D50 is 0.01 μm) is selected as the inactive inorganic filler, and its mass accounts for 10% of the total mass of the mixed slurry; KH570 silane coupling agent is selected as the coupling agent, and its mass accounts for 1% of the total mass of the in-situ polymerization precursor solution; at room temperature, the in-situ polymerization precursor solution, titanium dioxide inorganic filler and KH570 silane coupling agent are fully mixed to form a uniform mixed slurry.

[0181] (4) In-situ solidification process: In an argon atmosphere with a water and oxygen value of ≤0.1 ppm, 30 μL cm -2 The prepared mixed slurry is injected into a battery semi-finished product equipped with a glass fiber porous support membrane, a positive electrode sheet and a negative electrode sheet (the porous support membrane is located between the positive electrode sheet and the negative electrode sheet) with a filling amount (based on the area of ​​the porous support membrane), and reacted at 80°C for 12 hours to obtain a solid electrolyte and a solid-state battery (lithium-ion secondary battery).

[0182] Example 9

[0183] The solid electrolyte and solid-state battery are prepared as follows:

[0184] (1) Selection and preparation of porous support membrane: A porous organic insulating film made of cellulose fiber was selected as the support membrane. The porosity of the membrane was 93% and the thickness was 30 μm.

[0185] (2) Preparation of in-situ polymerization precursor solution: 1,3-dioxolane (DOL) was used as the polymerization monomer, LiTFSI was used as the electrolyte salt, and FEC was used as the additive. They were mixed in a mass ratio of 50:20:30, and 0.15% of aluminum trifluoromethanesulfonate by mass of DOL was added as a catalyst. Under the protection of argon, these components were fully mixed at room temperature.

[0186] (3) Preparation of mixed slurry: Lithium phosphorus sulfur chlorine solid electrolyte (Li6PS5Cl, D50 is 20μm) is selected as the active inorganic filler, and its mass accounts for 10% of the total mass of the mixed slurry; γ-aminopropyltriethoxysilane (KH550 silane coupling agent) is selected as the coupling agent, and its mass accounts for 2% of the total mass of the in-situ polymerization precursor solution; at room temperature, the in-situ polymerization precursor solution is fully mixed with the Li6PS5Cl inorganic filler and the KH550 silane coupling agent to form a uniform mixed slurry.

[0187] (4) In-situ solidification process: In an argon atmosphere with a water and oxygen value of ≤0.1 ppm, 10 μL cm -2The prepared mixed slurry is injected into a battery semi-finished product equipped with a cellulose fiber porous support membrane, a positive electrode sheet and a negative electrode sheet (the porous support membrane is located between the positive electrode sheet and the negative electrode sheet) with a filling amount (based on the area of ​​the porous support membrane), and reacted at 30°C for 48 hours to obtain a solid electrolyte and a solid-state battery (lithium-ion secondary battery).

[0188] The solid electrolyte in each embodiment and each comparative example is an in-situ solidified composite solid electrolyte.

[0189] The room temperature ionic conductivity of the solid electrolyte in each embodiment and each comparative example is tested as follows: by assembling a stainless steel (SS) ‖ solid electrolyte ‖ SS symmetric cell, the solid electrolyte is subjected to electrochemical impedance spectroscopy testing on a CHI 660E electrochemical workstation at room temperature, and the room temperature ionic conductivity of the solid electrolyte is calculated using the following formula:

[0190]

[0191] Where σ is the ionic conductivity of the solid electrolyte, in S cm -1 ; L is the thickness of the solid electrolyte, in cm; R b is the bulk impedance, in Ω; S is the area of ​​the solid electrolyte (also the contact area with SS), in cm 2 .

[0192] The contact angle of the porous support membrane in each embodiment and each comparative example is tested according to the following method: using a German Lauda Scientific LSA100 contact angle tester for testing, placing the porous support membrane on a contact angle testing platform, using the equipment's automatic titration system to drop a precursor solution on the porous support membrane, taking test photos, and measuring the contact angle using the goniometer method.

[0193] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0194] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims, and the description may be used to interpret the content of the claims.

Claims

1. A method for preparing a secondary battery, characterized in that: The steps include: Providing a semi-finished battery product including a positive electrode sheet, a negative electrode sheet and a porous support membrane, wherein the porous support membrane is arranged between the positive electrode sheet and the negative electrode sheet, and the porosity of the porous support membrane is greater than or equal to 70%; A mixed slurry containing a precursor solution, an inorganic filler and a coupling agent is injected into the battery semi-finished product and solidified so that the inorganic filler, the coupling agent and the solid electrolyte body are at least arranged in the pore structure of the porous support membrane to obtain the secondary battery containing a solid electrolyte; the mixed slurry is obtained by mixing the precursor solution, the inorganic filler and the coupling agent; the precursor solution contains a polymerized monomer and an electrolyte salt, the polymerized monomer is at least one of ethylene glycol dimethacrylate, vinyl ethylene carbonate and 1,3-dioxolane, the solid-liquid interface contact angle between the precursor solution and the porous support membrane in the secondary battery is 0~50°, the solid electrolyte body contains a polymer formed by the polymerized monomer and the electrolyte salt, and the mass of the coupling agent is 0.01%~10% of the mass of the precursor solution.

2. The preparation method according to claim 1, characterized in that: The preparation method satisfies at least one of the following conditions (1) to (2): (1) The curing process conditions include: a curing temperature of 25°C to 100°C and a curing time of 0.5h to 300h; (2) The mass proportion of the inorganic filler in the mixed slurry is 0.05% to 50%.

3. The preparation method according to any one of claims 1 to 2, characterized in that The solid electrolyte has at least one of the following characteristics (1) to (4): (1) The porosity of the porous support membrane is 70% to 99%; (2) The thickness of the porous support membrane is 1 μm to 200 μm; (3) The mass of the inorganic filler is 0.05% to 50% of the total mass of the solid electrolyte body, the inorganic filler and the coupling agent; (4) The precursor solution further comprises at least one of an initiator, a catalyst and an additive.

4. The preparation method according to any one of claims 1 to 2, characterized in that The solid electrolyte has at least one of the following characteristics (1) to (5): (1) The inorganic filler comprises at least one of an inorganic solid electrolyte material, an inorganic oxide, a silicate mineral material and a composite material thereof; (2) The average particle size D50 of the inorganic filler is 0.01 μm to 50 μm; (3) The coupling agent includes at least one of a silane coupling agent, a titanate coupling agent, an aluminate coupling agent, an aluminum zirconate coupling agent and an organic complex; (4) The electrolyte salt comprises at least one of a lithium-containing inorganic salt, a lithium-containing organic salt, a sodium-containing inorganic salt, a sodium-containing organic salt and a multi-salt complex; (5) The porous support membrane includes at least one of a porous organic insulating film and a porous inorganic insulating film, the material of the porous organic insulating film includes at least one of cellulose fiber, polypropylene fiber, polyethylene fiber, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyvinylidene fluoride-acrylonitrile copolymer, polyether sulfone, polyacrylonitrile, polyvinylidene chloride, polyimide, polyurethane, polyvinyl chloride, polyvinyl carbonate and polypropylene carbonate, and the material of the porous inorganic insulating film includes at least one of glass fiber, boron fiber, ceramic fiber, silicon dioxide, aluminum oxide and titanium dioxide.

5. The preparation method according to claim 4, characterized in that: The solid electrolyte has at least one of the following characteristics (1) to (3): (1) The inorganic solid electrolyte material includes at least one of an oxide solid electrolyte, a sulfide solid electrolyte, a halide solid electrolyte, a sulfide solid electrolyte, an oxyhalide solid electrolyte, and a composite solid electrolyte thereof; (2) The inorganic oxide comprises at least one of silicon dioxide, titanium dioxide and aluminum oxide; (3) The silicate mineral material includes at least one of rectorite, montmorillonite, kaolin, mica powder, talc, attapulgite, halloysite, sepiolite, vermiculite and wollastonite.

6. The preparation method according to claim 3, characterized in that: The solid electrolyte has at least one of the following characteristics (1) to (3): (1) The initiator comprises at least one of an azo initiator, an organic peroxide initiator, an inorganic peroxide initiator, a redox initiator and an ionic initiator; (2) The catalyst comprises at least one of a Lewis acid catalyst, a cationic catalyst, an anionic catalyst, a coordination catalyst and a rare earth metal catalyst; (3) The additive includes at least one of fluoroethylene carbonate, succinonitrile, polyethylene glycol and polyethylene glycol dimethyl ether.

7. A secondary battery, characterized in that: The method is prepared according to any one of claims 1 to 6.

8. An electrical device, characterized in that: A secondary battery comprising the secondary battery according to claim 7.

Citation Information

Patent Citations

  • High-strength solid electrolyte membrane and preparation method and application thereof

    CN113363561A

  • Non-woven cloth increasing micropore polymer diaphragm and usage as well as preparation method thereof

    CN101226994A

  • Preparation method of ceramic grafted diaphragm and application of ceramic grafted diaphragm in lithium battery

    CN104600229A

  • Lithium-ion battery diaphragm and preparation method thereof

    CN105140451A

  • Inorganic coated bacterial cellulose porous thin film and preparation method thereof

    CN106450115A