A kind of adsorbent and its preparation method and application

The combination of biomass-oxide substrates and magnesium salts and halogen salts is prepared through interface induction to form high-efficiency alumina adsorbents, which solves the shortcomings of activated alumina adsorbents in high concentration of moisture and compressed gas drying, and improves adsorption performance and structural stability.

CN118594493BActive Publication Date: 2024-11-19HANGZHOU JIALONG AIR EQUIP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411083583.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-19
Estimated Expiration
2044-08-08

AI Technical Summary

Technical Problem

The existing activated alumina adsorbents are inefficient when treating high concentration water molecules and need to be replaced frequently. The structural strength is insufficient during compressed air drying, resulting in pore structure collapse and affecting adsorption performance.

Method used

The biomass-oxide substrate is prepared by interface induction, and alumina-based adsorbent is formed by pretreatment and pyrolysis of microcrystalline cellulose, combining magnesium salts and halogen salts to enhance the support and hygroscopicity of the pores, and impregnated by high-temperature acid liquids. and freeze-drying to adjust the pore structure.

Benefits of technology

It improves the affinity and stability of the adsorbent to water molecules, reduces the regeneration temperature, extends the service life, and provides better structural support in compressed gas drying, significantly improving the adsorption effect and regeneration efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention belongs to the technical field of adsorbent preparation, and specifically relates to an adsorbent and its preparation method and application. The method comprises: 1) taking a polysaccharide raw material and an alkali solution and mixing them evenly, after heating, filtering and drying, adding a solvent, an aluminum salt, and a magnesium salt and mixing them evenly, filtering and drying, and then performing a pyrolysis pretreatment to obtain a pyrolysis product; 2) adding the pyrolysis product to a lithium salt solution for a mixed reaction, filtering, washing, drying, and then adding it to a calcium salt solution for a mixed reaction to obtain an intermediate product, and sequentially performing a high-temperature treatment, an acid solution immersion treatment, filtering, washing, and drying on the intermediate product to obtain a substrate; 3) dispersing the substrate in a solvent, adding an inorganic acid ester and an acid solution and mixing them evenly, and freeze-drying to obtain an adsorbent. The adsorbent prepared by the present invention can stably store water, has long-term and stable adsorption, a low regeneration temperature, can be reversely adsorbed at a lower temperature, and has good stability, and is suitable for drying and dehydrating compressed gases.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of adsorbent preparation, and specifically relates to an adsorbent and a preparation method and application thereof. Background Art

[0002] At present, activated alumina is commonly used for water removal by adsorption. The preparation methods of activated alumina include hydrolysis method, precipitation method, etc. In the prior art, activated alumina cannot handle high concentrations of water molecules, and related products need to be replaced frequently. Moreover, the regeneration efficiency of activated alumina adsorbent is significantly reduced after being used for a period of time. Based on the limitations of the cost and adsorption performance of activated alumina adsorbent, the field urgently needs to develop a new and more effective activated alumina adsorbent.

[0003] A porous structure with multiple contact active sites is considered to be a key condition for the development of efficient adsorbents. In this field, alumina is used as a protective layer to be loaded on substrates such as zeolite and resin to extend the service life of the adsorbent and the service life of the substrate. Based on the protective layer method, activated alumina is obtained by high-temperature treatment of thermally activated alumina alkaline hydrate containing more than 50 wt% of bainite phase. Above 300 °C, low-temperature phase alumina (η-Al2O3, γ-Al2O3) is formed. The adsorbent has the advantages of large specific surface area, rich surface sites, and dense pores. The adsorbent is then deposited to obtain a larger static capacity. However, this method cannot guarantee the relative content of η-Al2O3 and γ-Al2O3.

[0004] In addition, the adsorption capacity of activated alumina is improved by chemically modifying the adsorbent surface with acid and alkali in this field, such as regulating the concentration of acid and base sites and the reactivity of hydroxyl groups on the surface of alumina, introducing sulfuric acid during the preparation process, and based on the fact that γ-Al2O3 has abundant Bronsted acid sites and effective Lewis acid sites, it was found through testing that the dynamic capacity of the product is comparable to that of bainite-based adsorbents, and the static capacity far exceeds that of bainite-based adsorbents, but its pore size is significantly reduced. Moreover, the environmental humidity affects the active state of the acid-base modified sites on the adsorbent surface, thereby affecting the static capacity.

[0005] In addition, when drying and removing water in compressed air, the existing alumina desiccant has insufficient structural support strength. Since the adsorption drying process of water vapor easily forms local pressure differences, and the ambient pressure is relatively high when drying in compressed gas, the negative impact of the local pressure difference is amplified, and the pore channel structure may collapse due to compression. Summary of the invention

[0006] In order to solve the problems of insufficient water absorption of activated alumina, its own instability, and insufficient structural strength when used as a desiccant in compressed gas, the present invention proposes an adsorbent and a preparation method and application thereof.

[0007] The objects of the present invention are:

[0008] 1. Improve the affinity of the adsorbent to water;

[0009] 2. Improve the stable storage capacity of the adsorbent for water and ensure stable adsorption of the adsorbent;

[0010] 3. Reduce the regeneration temperature of the adsorbent and extend its service life;

[0011] 4. Improve the structural support strength of the adsorbent to make it more effective for compressed gas drying.

[0012] To achieve the above objectives, the present invention adopts the following technical solutions.

[0013] A method for preparing an adsorbent,

[0014] The method comprises:

[0015] 1) Mix the polysaccharide raw material and alkali solution evenly, heat, filter and dry, then add the solvent, aluminum salt and magnesium salt and mix evenly, filter and dry, perform pyrolysis pretreatment and obtain pyrolysis products;

[0016] 2) adding the pyrolysis product to a lithium salt solution for a mixed reaction, filtering, washing, and drying, and then adding it to a calcium salt solution for a mixed reaction to obtain an intermediate product, and sequentially subjecting the intermediate product to a high temperature treatment, an acid solution impregnation treatment, filtering, washing, and drying to obtain a substrate;

[0017] 3) Disperse the substrate in a solvent, add inorganic acid ester and acid solution, mix evenly, and obtain the adsorbent by freeze-drying.

[0018] As a preference,

[0019] Step 1) the polysaccharide raw material is microcrystalline cellulose;

[0020] Step 1) The dosage of the alkali solution is 10-15 mL / g polysaccharide raw material, and the preparation method is as follows:

[0021] Take sodium sulfite and sodium hydroxide in a mass ratio of 1: (2-2.2), add 15-25 mL of water per gram of sodium sulfite and mix evenly;

[0022] In step 1), the heating is carried out at 80-90°C and kept at a constant temperature for 5-6 hours.

[0023] As a preference,

[0024] Step 1) the solvent is anhydrous ethanol, and the amount thereof is 5-10 mL / g polysaccharide raw material;

[0025] Step 1) the aluminum salt is aluminum chloride, and its usage is 1.3-1.6 g / g polysaccharide raw material;

[0026] Step 1) the magnesium salt is magnesium chloride, and its dosage is 0.1-0.15 g / g polysaccharide raw material;

[0027] Step 1) The pyrolysis pretreatment is carried out in an atmosphere with an oxygen content of ≤2%VOL or in an inert gas protective atmosphere at 300-350°C for 10-15 min.

[0028] As a preference,

[0029] Step 2) the lithium salt solution is a lithium chloride aqueous solution with a concentration of 22 to 28 wt % and an amount of 3 to 5 mL / g of pyrolysis product;

[0030] The reaction time of adding the mixture into the lithium salt solution for the mixed reaction is 6 to 12 hours.

[0031] As a preference,

[0032] Step 2) the calcium salt solution is a calcium chloride aqueous solution with a concentration of 7 to 13 wt % and an amount of 3 to 5 mL / g of pyrolysis product;

[0033] The reaction time of adding to the calcium salt solution for mixed reaction is 6 to 12 hours.

[0034] As a preference,

[0035] Step 2) The high temperature treatment is carried out at 550-600°C for 2-2.5 hours;

[0036] In step 2), the acid immersion treatment is carried out at 100°C, using hydrochloric acid with a concentration of 1 to 2 mol / L to immerse the intermediate product for a treatment time of 12 to 14 hours.

[0037] As a preference,

[0038] Step 3) The solvent is anhydrous ethanol, and 25 to 30 mL of the solvent is added per gram of substrate;

[0039] Step 3) the inorganic acid ester is ethyl silicate, and 0.5 to 0.8 mL of the inorganic acid ester is added per gram of substrate;

[0040] Step 3) the acid solution is acetic acid, and 0.1 to 0.2 mL of the acid solution is added per gram of substrate;

[0041] Step 3) The immersion treatment time is 30 to 60 minutes.

[0042] As a preference,

[0043] Step 3) The freeze drying is carried out at -60 to -50°C and a vacuum degree lower than 0.1 mbar for 48 to 52 hours.

[0044] An adsorbent,

[0045] The adsorbent is an alumina-based adsorbent, and the alumina forms a hollow structure oxide.

[0046] Application of an adsorbent,

[0047] The adsorbent is used to dry compressed gas.

[0048] Generally speaking, changes in phase composition, texture characteristics and surface acid-base properties can significantly affect the adsorption capacity of activated alumina. In order to obtain a porous structure with multiple contact active sites, in the technical solution of the present invention, an interface induction is used to prepare a biomass-oxide substrate. The present invention first pre-treats microcrystalline cellulose, removes its impurities and bound water by alkali solution impregnation and heat treatment. Then the microcrystalline cellulose is immersed in a mixed aqueous solution of aluminum salt and magnesium salt to form an aluminum-magnesium-biomass interface. The aluminum precursor is anchored on the microcrystalline cellulose. Microcrystalline cellulose provides a large number of oxygen-containing groups, which are conducive to bonding metal cations and inducing the nucleation growth of metal oxides. If proteins or amino acids are used as the core, the inherent functional groups of proteins can well complex metals and provide a complex molecular skeleton, while the molecular diameter of amino acids is small, which helps to form hollow structure oxides. However, the separation and purification process of soft templates such as proteins and amino acids is complicated and easy to aggregate, which is not conducive to the separation of aluminum-magnesium-carbon, causing the pores to be blocked, thereby resulting in poor application effect of adsorbing water.

[0049] The present invention uses relatively low temperature to carry out pyrolysis, and carbonization ensures that the microcrystalline cellulose is converted into carbonaceous material. In the pyrolysis process, aluminum chloride is thermally decomposed and contacts oxygen in the environment, so that the aluminum chloride is converted into aluminum oxide. At the same time, the present invention utilizes the structural characteristics of microcrystalline cellulose itself, so that a fibrous structure with clear lines and burrs is formed in the alumina pores. However, this method has reduced controllability of the pore structure. In order to enhance the support of the alumina pores, the present invention adds magnesium salts to enhance the hydrogen bond interaction between Al-hydroxyl active species and biomass. The formation of magnesium oxide during the pyrolysis process promotes the reduction of grain boundary size, increases grain boundary density, promotes the refinement of alumina grains, and significantly improves the strength of the alumina pores.

[0050] After testing, the pores are more solid, and magnesium and aluminum are evenly dispersed in the substrate. In addition, the hard template method is conducive to the interaction and nucleation growth of oxygen-containing groups of microcrystalline cellulose with Al3+ and Mg2+, and the replication of the structure of microcrystalline cellulose. Otherwise, aluminum oxide and magnesium oxide are unevenly distributed, and the uniformity of their morphology and size cannot be controlled, thus affecting the final adsorption effect.

[0051] Most importantly, the gas can pass through the adsorbent through radial transmission channels, making it pass faster, which is conducive to the formation of capillary forces and surface tension to ensure the stable adsorption of water molecules. After the pyrolysis process, the interaction between alumina and carbon is eliminated. This method makes the substrate have more abundant pores and effectively adjusts the porosity and pore structure of the substrate. After characterization, the interfacial combustion induced a higher aromaticity of carbon on the surface of alumina, which indicates that the carbon is combined together, which is conducive to the removal of carbon in the subsequent steps.

[0052] Moreover, during the pyrolysis process, excessively high temperatures will cause the oxygen-containing groups on the microcrystalline cellulose to decompose rapidly, and due to the high temperature, the material is unevenly dehydrogenated, deoxygenated and dehydrated, and AI3+ exhibits octahedral coordination, pentahedral coordination, and tetrahedral coordination. Among them, the intensity of the AI3+ octahedral coordination peak is much lower.

[0053] In order to improve the affinity of the adsorbent to water molecules, the present invention uses a substrate to compound lithium chloride and calcium chloride. Strongly hydrophilic halogen salts such as Li+ and Ca2+ can significantly improve the hygroscopicity of the adsorbent, but in a high humidity environment, the halogen salt will undergo liquefaction and loss, resulting in a decrease in hygroscopicity. The present invention combines aluminum oxide with halogen salts, so that Li+ and Ca2+ are fully exchanged with Na+ on the pore wall, the hydrophilicity of the adsorbent is enhanced, the rate at which water vapor passes through the adsorbent is enhanced, and some water molecules are adsorbed to form bound water. The introduction of Li+ can synergistically enhance the electronic interaction between hydroxyl and ester groups, destroy hydrogen bonds and particle structures, reduce the crystallinity of inorganic salt hydrates, and avoid pore blockage. The substrate has a limited loading capacity for lithium chloride and calcium chloride. In order to ensure that the adsorbent has a good affinity for water molecules, combined with economic benefits, the present invention controls the amount of water-absorbing metal salts.

[0054] Furthermore, in order to improve the activity of the adsorbent itself, the present invention induces the residual substances of the polysaccharide raw material to the surface layer of the grain boundary through high temperature and acid leaching treatment, which is conducive to removing the residual substances during acid leaching, and at the same time, the hygroscopic metal salt diffuses into the grain boundary, which is conducive to enhancing the hydrophilicity of the substrate. Among them, by regulating the temperature of high temperature treatment, the alumina substrate of the target crystal form can be constructed. If the treatment temperature is too low or too high, it will not be possible to obtain γ-Al2O3 with an open lattice structure with strong support, high porosity and large skeleton pore size.

[0055] The present invention modifies the surface of the substrate by ethyl silicate, and forms a sol on the surface of the matrix pore channel by infiltration before the freeze-drying process, and obtains a nanostructure with capillary characteristics after freeze-drying. The multi-level capillary structure enables the adsorbent to form a strong adsorption effect on water molecules. In a high humidity environment, the saturated adsorption capacity of the adsorbent of the present invention is much higher than that of commercially available adsorbents, and has excellent saturated adsorption capacity. If there is no protection of ethyl silicate, the active sites of the secondary structure of aluminum oxide are easily lost in a high temperature environment. In an environment with a relative humidity of less than 15%, the adsorbent adsorbs water molecules, and the water molecules are filled into the micropores of the material. At this time, the adsorption capacity of the adsorbent depends on the richness of the capillary structure of the adsorbent. In an environment with a relative humidity of between 15% and 40%, water molecules will hydrogen bond with water molecules around the adsorption sites in the pores to further form water molecule clusters. At this time, the sufficient space provided by the adsorbent enables it to have excellent saturated adsorption capacity, and the capillary structure and hydrophilic adsorption sites enable the adsorbent to have long-term dehumidification ability. In addition, experiments have found that by heating the adsorbent at a relatively low temperature, a certain amount of bound water can be released again, resulting in an adsorbent that still has a good adsorption effect.

[0056] The beneficial effects of the present invention are as follows:

[0057] (1) The adsorbent prepared by the present invention has a high affinity for water;

[0058] (2) The adsorbent prepared by the present invention can stably store water and has long-lasting and stable adsorption;

[0059] (3) The adsorbent prepared by the present invention has a low regeneration temperature and can be reversely adsorbed at a lower temperature while maintaining a good adsorption effect;

[0060] (4) The adsorbent prepared by the present invention has a stable supporting structure and is suitable for drying and dehydrating compressed gas. DETAILED DESCRIPTION

[0061] The present invention is further described in detail below in conjunction with specific embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.

[0062] Unless otherwise specified, the raw materials used in the examples of the present invention are all commercially available or available to those skilled in the art; unless otherwise specified, the methods used in the examples of the present invention are all methods known to those skilled in the art.

[0063] Example 1

[0064] A method for preparing an adsorbent, the method comprising:

[0065] 1) 5 g of sodium sulfite, 11 g of sodium hydroxide and 100 mL of water were mixed evenly to obtain an alkali solution, 10 g of microcrystalline cellulose was added and mixed evenly, and the mixture was kept at 80 °C for 6 h. After filtering and drying, the solid product was obtained. 50 mL of anhydrous ethanol, 13 g of aluminum chloride and 1 g of magnesium chloride were added and mixed evenly, and the solid product was filtered and dried. The solid product was pyrolyzed in a nitrogen atmosphere at 350 °C for 10 min to obtain a pyrolysis product;

[0066] 2) adding the pyrolysis product to a 24 wt% lithium chloride aqueous solution, the amount of which is 3 mL / g of the pyrolysis product, mixing and stirring for 8 h, filtering, washing, and drying, and then adding it to a 10 wt% calcium chloride aqueous solution, the amount of which is 3 mL / g of the pyrolysis product, mixing and stirring for 8 h to obtain an intermediate product, placing the intermediate product at 550 ° C, keeping the temperature constant for 2.5 h, immersing the material in 2 mol / L hydrochloric acid at 100 ° C, treating for 12 h, filtering, washing, and drying to obtain a substrate;

[0067] 3) Add 25 mL of anhydrous ethanol per gram of substrate to ensure that the substrate is completely dispersed in the anhydrous ethanol, add 0.5 mL of ethyl silicate per gram of substrate, add 0.1 mL of acetic acid per gram of substrate and mix well, immerse for 60 min, and treat for 48 h at -60 °C and a vacuum degree of less than 0.1 mbar to obtain an adsorbent.

[0068] The adsorbent prepared in this example was characterized and its performance tested, wherein the basic characterization and performance tests are specifically as follows.

[0069] 1. Characterization:

[0070] The nitrogen adsorption-desorption method was used to test the porosity and other parameters of the adsorbent; the flow rate of gas through the adsorbent was measured by the steady-state method, and the permeability was calculated by the Ergun model;

[0071] 2. Performance test:

[0072] The adsorbent was placed in a sealed environment with a room temperature of 30 °C and a relative humidity of 75%. The air pressure in the sealed environment was normal pressure (1.0±0.05 atm). A saturated moisture absorption experiment was carried out with an insufficient amount of the adsorbent prepared in this example (i.e., ensuring that the relative humidity was still ≥30% after 24 hours of constant temperature). The constant temperature was maintained for 24 hours, and the adsorption rate and saturated moisture absorption of the adsorbent were detected. Based on the gas dehumidification experiment, the adsorbent was placed at 100 °C and kept at a constant temperature for 8 hours. The saturated moisture absorption experiment was repeated 15 times. The results of the saturated moisture absorption were compared to calculate its regeneration efficiency.

[0073] The results are as follows.

[0074] Porosity (%) Permeability (m2) Adsorption rate g / (g·min) Saturated moisture absorption (g / g) Regeneration efficiency (%) 94.8 10-12 0.0242 1.594 97

[0075] Gas can pass through the adsorbent through the radial transmission channel, making it pass faster, which is conducive to the formation of capillary force and surface tension to ensure stable adsorption of water molecules. After characterization, the surface carbonaceous aromaticity of the interfacial combustion-induced alumina is higher, and after testing, the alumina content in the substrate exceeds 85 wt%. Moreover, by high temperature and acid leaching treatment, impurities are lured to the surface of the grain boundary, and the impurities are removed during acid leaching. At the same time, hygroscopic metal salts diffuse into the grain boundary, which is conducive to enhancing the hydrophilicity of the substrate. After experiments, it can be analyzed that the adsorbent prepared by the present invention has a high porosity, rapid adsorption, good adsorption effect, and high regeneration efficiency after reverse adsorption by heating the adsorbent at a lower temperature.

[0076] On the basis of the above characterization, the present invention also conducts a pressurized saturated moisture absorption experiment on the basis of the saturated moisture absorption experiment, increases the air pressure in the sealed environment to pressurized compressed gas (12.0±0.2 atm), and maintains the temperature at 30°C and the relative humidity at 75%. The adsorbent prepared in this example is subjected to a saturated moisture absorption experiment (i.e., ensuring that the relative humidity is still ≥30% after 24 hours of constant temperature), and the constant temperature is maintained for 24 hours to detect the adsorption rate and saturated moisture absorption of the adsorbent; based on the gas dehumidification experiment, the adsorbent is placed at 100°C and kept at a constant temperature for 8 hours, and the pressurized saturated moisture absorption experiment is repeated 30 times, and the results are compared to calculate the regeneration efficiency. The results of the pressurized saturated moisture absorption experiment show that the initial adsorption rate is about 0.0228 g / (g·min), the initial saturated moisture absorption is 1.578 g / g adsorbent, and the regeneration efficiency reaches 93%. This shows that the high-pressure atmosphere does cause certain damage to the activated alumina, especially the local pressure difference caused by the moisture absorption process may cause damage to the structure of the activated alumina, but the degree of damage is low. This also shows that the adsorbent of the present invention has a good compressed gas drying effect.

[0077] Example 2

[0078] A method for preparing an adsorbent, the method comprising:

[0079] 1) 5 g of sodium sulfite, 11 g of sodium hydroxide and 100 mL of water were mixed evenly to obtain an alkali solution, 10 g of microcrystalline cellulose was added and mixed evenly, and the mixture was kept at 80 °C for 6 h. After filtering and drying, the solid product was obtained. 50 mL of anhydrous ethanol, 13 g of aluminum chloride and 1.3 g of magnesium chloride were added and mixed evenly, and the solid product was taken out after filtering and drying. The solid product was pyrolyzed in a nitrogen atmosphere at 350 °C for 10 min to obtain a pyrolysis product;

[0080] 2) adding the pyrolysis product to a 24 wt% lithium chloride aqueous solution, the amount of which is 3 mL / g of the pyrolysis product, mixing and stirring for 8 h, filtering, washing, and drying, and then adding it to a 10 wt% calcium chloride aqueous solution, the amount of which is 3 mL / g of the pyrolysis product, mixing and stirring for 8 h to obtain an intermediate product, placing the intermediate product at 550 ° C, keeping the temperature constant for 2.5 h, immersing the material in 2 mol / L hydrochloric acid at 100 ° C, treating for 12 h, filtering, washing, and drying to obtain a substrate;

[0081] 3) Add 25 mL of anhydrous ethanol per gram of substrate to ensure that the substrate is completely dispersed in the anhydrous ethanol, add 0.5 mL of ethyl silicate per gram of substrate, add 0.1 mL of acetic acid per gram of substrate and mix well, immerse for 60 min, and treat for 48 h at -60 °C and a vacuum degree of less than 0.1 mbar to obtain an adsorbent.

[0082] The adsorbent prepared in this example was subjected to the same characterization and performance testing as in Example 1, and the results are as follows.

[0083] Porosity (%) Permeability (m2) Adsorption rate g / (g·min) Saturated moisture absorption (g / g) Regeneration efficiency (%) 95.1 10-12 0.0265 1.598 98

[0084] In this case, the amount of magnesium salt was increased, and the hydrogen bond interaction between Al-hydroxyl active species and biomass was enhanced. The magnesium oxide formed during the pyrolysis process promoted the reduction of grain boundary size, increased grain boundary density, and promoted the refinement of alumina grains, which significantly improved the strength of alumina channels. The fibrous structure with burrs in the alumina channels was clear, and the adsorption effect was enhanced.

[0085] The results of the pressurized saturated moisture absorption test showed that the initial adsorption rate was about 0.0233 g / (g·min), the initial saturated moisture absorption was 1.585 g / g adsorbent, and the regeneration efficiency reached 95%. This shows that the increase in the amount of magnesium salt strengthens the strength of the alumina pores, further improving its moisture absorption performance and compressive resistance in compressed gas.

[0086] Example 3

[0087] A method for preparing an adsorbent, the method comprising:

[0088] 1) 5 g of sodium sulfite, 11 g of sodium hydroxide and 100 mL of water were mixed evenly to obtain an alkali solution, 10 g of microcrystalline cellulose was added and mixed evenly, and the mixture was kept at 80 °C for 6 h. After filtering and drying, the solid product was obtained. 50 mL of anhydrous ethanol, 13 g of aluminum chloride and 1.5 g of magnesium chloride were added and mixed evenly, and the solid product was filtered and dried. The solid product was pyrolyzed in a nitrogen atmosphere at 350 °C for 10 min to obtain a pyrolysis product;

[0089] 2) adding the pyrolysis product to a 24 wt% lithium chloride aqueous solution, the amount of which is 3 mL / g of the pyrolysis product, mixing and stirring for 8 h, filtering, washing, and drying, and then adding it to a 10 wt% calcium chloride aqueous solution, the amount of which is 3 mL / g of the pyrolysis product, mixing and stirring for 8 h to obtain an intermediate product, placing the intermediate product at 550 ° C, keeping the temperature constant for 2.5 h, immersing the material in 2 mol / L hydrochloric acid at 100 ° C, treating for 12 h, filtering, washing, and drying to obtain a substrate;

[0090] 3) Add 25 mL of anhydrous ethanol per gram of substrate to ensure that the substrate is completely dispersed in the anhydrous ethanol, add 0.5 mL of ethyl silicate per gram of substrate, add 0.1 mL of acetic acid per gram of substrate and mix well, immerse for 60 min, and treat for 48 h at -60 °C and a vacuum degree of less than 0.1 mbar to obtain an adsorbent.

[0091] The adsorbent prepared in this example was subjected to the same characterization and performance testing as in Example 1, and the results are as follows.

[0092] Porosity (%) Permeability (m2) Adsorption rate g / (g·min) Saturated moisture absorption (g / g) Regeneration efficiency (%) 93.6 10-13 0.0228 1.581 94

[0093] In this example, the amount of magnesium salt is further increased to form magnesium oxide, which blocks some pores and causes a decrease in the adsorption effect. Combining Examples 1 to 3, it can be analyzed that in a high humidity environment, the adsorbent of the present invention has a high saturation adsorption capacity and an excellent saturation adsorption capacity.

[0094] The same pressurized saturated moisture absorption test was carried out. The results showed that the initial adsorption rate under the pressurized saturated moisture absorption test was about 0.0209 g / (g·min), the initial saturated moisture absorption was 1.556 g / g adsorbent, and the regeneration efficiency reached 90%. This shows that the actual high-pressure resistance capacity is weakened after the excessive magnesium salt causes the pores to be blocked, especially when some pores are blocked, they are easily affected by the high pressure of compressed gas, and the structure collapses due to the pressure difference between the inside and outside of the local structure.

[0095] Comparative Example 1

[0096] A method for preparing an adsorbent, the method comprising:

[0097] 1) Take 5 g of sodium sulfite, 11 g of sodium hydroxide, and 100 mL of water, mix them evenly to obtain an alkali solution, add 10 g of glutamic acid and mix them evenly, keep the temperature at 80 °C for 6 h, filter and dry the solid product, add 50 mL of anhydrous ethanol, 13 g of aluminum chloride, and 1.3 g of magnesium chloride, mix them evenly, filter and dry the solid product, and pyrolyze it in a nitrogen atmosphere at 350 °C for 10 min to obtain a pyrolysis product;

[0098] 2) adding the pyrolysis product to a 24 wt% lithium chloride aqueous solution, the amount of which is 3 mL / g of the pyrolysis product, mixing and stirring for 8 h, filtering, washing, and drying, and then adding it to a 10 wt% calcium chloride aqueous solution, the amount of which is 3 mL / g of the pyrolysis product, mixing and stirring for 8 h to obtain an intermediate product, placing the intermediate product at 550 ° C, keeping the temperature constant for 2.5 h, immersing the material in 2 mol / L hydrochloric acid at 100 ° C, treating for 12 h, filtering, washing, and drying to obtain a substrate;

[0099] 3) Add 25 mL of anhydrous ethanol per gram of substrate to ensure that the substrate is completely dispersed in the anhydrous ethanol, add 0.5 mL of ethyl silicate per gram of substrate, add 0.1 mL of acetic acid per gram of substrate and mix well, immerse for 60 min, and treat for 48 h at -60 °C and a vacuum degree of less than 0.1 mbar to obtain an adsorbent.

[0100] The adsorbent prepared in this example was subjected to the same characterization and performance testing as in Example 1, and the results are as follows.

[0101] Porosity (%) Permeability (m2) Adsorption rate g / (g·min) Saturated moisture absorption (g / g) Regeneration efficiency (%) 91.6 10-14 0.0212 1.561 91

[0102] In this case, glutamic acid was used as the biomass template. Due to its small molecular diameter, the adsorbent formed larger pores. However, due to the complex biomass separation and purification process, it is easy to aggregate, which is not conducive to the separation of aluminum-magnesium-carbon, resulting in pore blockage, and the gas cannot be quickly transmitted through the radial channel. Its passing rate is low, resulting in poor application effect of moisture adsorption.

[0103] The same pressurized saturated moisture absorption experiment was carried out. The results showed that the initial adsorption rate under the pressurized saturated moisture absorption experiment was about 0.0201 g / (g·min), the initial saturated moisture absorption was 1.453 g / g adsorbent, and the regeneration efficiency reached 87%. This is also due to the blockage of some pores, resulting in a small local air pressure in the original structure, which is easy to cause a pressure difference with the high-pressure environment, resulting in structural collapse and damage.

[0104] Comparative Example 2

[0105] A method for preparing an adsorbent, the method comprising:

[0106] 1) Take 50 mL of anhydrous ethanol, 13 g of aluminum chloride, and 1.3 g of magnesium chloride and mix them evenly. After filtering and drying, take the solid product and pyrolyze it in a nitrogen atmosphere at 350 °C for 10 min to obtain the pyrolysis product;

[0107] 2) adding the pyrolysis product to a 24 wt% lithium chloride aqueous solution, the amount of which is 3 mL / g of the pyrolysis product, mixing and stirring for 8 h, filtering, washing, and drying, and then adding it to a 10 wt% calcium chloride aqueous solution, the amount of which is 3 mL / g of the pyrolysis product, mixing and stirring for 8 h to obtain an intermediate product, placing the intermediate product at 550 ° C, keeping the temperature constant for 2.5 h, immersing the material in 2 mol / L hydrochloric acid at 100 ° C, treating for 12 h, filtering, washing, and drying to obtain a substrate;

[0108] 3) Add 25 mL of anhydrous ethanol per gram of substrate to ensure that the substrate is completely dispersed in the anhydrous ethanol, add 0.5 mL of ethyl silicate per gram of substrate, add 0.1 mL of acetic acid per gram of substrate and mix well, immerse for 60 min, and treat for 48 h at -60 °C and a vacuum degree of less than 0.1 mbar to obtain an adsorbent.

[0109] The adsorbent prepared in this example was subjected to the same characterization and performance testing as in Example 1, and the results are as follows.

[0110] Porosity (%) Permeability (m2) Adsorption rate g / (g·min) Saturated moisture absorption (g / g) Regeneration efficiency (%) 84.7 10-16 0.0149 1.429 81

[0111] In the present invention, the oxygen-containing groups provided by microcrystalline cellulose bond to metal cations, interact with Al3+ and Mg2+, form nuclei and grow, and replicate the structure of microcrystalline cellulose. However, this example does not use the biomass hard template method, otherwise, aluminum oxide and magnesium oxide are unevenly distributed, the uniformity of their morphology and size cannot be controlled, and the adsorption effect is significantly reduced.

[0112] The same pressurized saturated moisture absorption experiment was carried out. The results showed that the initial adsorption rate under the pressurized saturated moisture absorption experiment was about 0.0133 g / (g·min), the initial saturated moisture absorption was 1.410 g / g adsorbent, and the regeneration efficiency reached 79%. This shows that although the adsorption performance itself is weak, due to the enhancement of magnesium and the fact that the structure of the adsorbent prepared in this example does not produce complex pores, although it leads to a decrease in adsorption rate and moisture absorption, it also improves the stability of its structure to a certain extent.

[0113] Comparative Example 3

[0114] A method for preparing an adsorbent, the method comprising:

[0115] 1) 5 g of sodium sulfite, 11 g of sodium hydroxide and 100 mL of water were mixed evenly to obtain an alkali solution, 10 g of microcrystalline cellulose was added and mixed evenly, and the mixture was kept at 80 °C for 6 h. After filtering and drying, the solid product was obtained. 50 mL of anhydrous ethanol, 13 g of aluminum chloride and 1.3 g of magnesium chloride were added and mixed evenly, and the solid product was filtered and dried. The solid product was pyrolyzed in a nitrogen atmosphere at 400 °C for 10 min to obtain a pyrolysis product;

[0116] 2) adding the pyrolysis product to a 24 wt% lithium chloride aqueous solution, the amount of which is 3 mL / g of the pyrolysis product, mixing and stirring for 8 h, filtering, washing, and drying, and then adding it to a 10 wt% calcium chloride aqueous solution, the amount of which is 3 mL / g of the pyrolysis product, mixing and stirring for 8 h to obtain an intermediate product, placing the intermediate product at 550 ° C, keeping the temperature constant for 2.5 h, immersing the material in 2 mol / L hydrochloric acid at 100 ° C, treating for 12 h, filtering, washing, and drying to obtain a substrate;

[0117] 3) Add 25 mL of anhydrous ethanol per gram of substrate to ensure that the substrate is completely dispersed in the anhydrous ethanol, add 0.5 mL of ethyl silicate per gram of substrate, add 0.1 mL of acetic acid per gram of substrate and mix well, immerse for 60 min, and treat for 48 h at -60 °C and a vacuum degree of less than 0.1 mbar to obtain an adsorbent.

[0118] The adsorbent prepared in this example was subjected to the same characterization and performance testing as in Example 1, and the results are as follows.

[0119] Porosity (%) Permeability (m2) Adsorption rate g / (g·min) Saturated moisture absorption (g / g) Regeneration efficiency (%) 92.4 10-15 0.0211 1.467 86

[0120] Too high a pyrolysis temperature will cause the oxygen-containing groups on the microcrystalline cellulose to decompose rapidly. In addition, due to the high temperature, the material is unevenly dehydrogenated, deoxygenated and dehydrated. AI3+ exhibits a variety of coordination forms such as octahedral coordination, pentahedral coordination, and tetrahedral coordination, resulting in incomplete performance and poor adsorbent activity, which significantly reduces its adsorption effect.

[0121] The same pressurized saturated moisture absorption test was carried out. The results showed that the initial adsorption rate under the pressurized saturated moisture absorption test was about 0.0168 g / (g·min), the initial saturated moisture absorption was 1.431 g / g adsorbent, and the regeneration efficiency reached 81%. Compared with Comparative Example 1, although this example should also have the strengthening effect of magnesium, it did not produce a more densely stacked structure like Comparative Example 1, but a multi-porous structure formed with the cooperation of microcrystalline cellulose. However, improper treatment in the subsequent pyrolysis process caused the structure to change and the strength to weaken, weakening the strengthening effect of magnesium, thereby significantly reducing its high pressure resistance.

[0122] Comparative Example 4

[0123] A method for preparing an adsorbent, the method comprising:

[0124] 1) 5 g of sodium sulfite, 11 g of sodium hydroxide and 100 mL of water were mixed evenly to obtain an alkali solution, 10 g of microcrystalline cellulose was added and mixed evenly, and the mixture was kept at 80 °C for 6 h. After filtering and drying, the solid product was obtained. 50 mL of anhydrous ethanol, 13 g of aluminum chloride and 1.3 g of magnesium chloride were added and mixed evenly, and the solid product was taken out after filtering and drying. The solid product was pyrolyzed in a nitrogen atmosphere at 350 °C for 10 min to obtain a pyrolysis product;

[0125] 2) Keep the temperature constant at 550 °C for 2.5 h, immerse the pyrolysis product in 2 mol / L hydrochloric acid at 100 °C for 12 h, filter, wash and dry to obtain the substrate;

[0126] 3) Add 25 mL of anhydrous ethanol per gram of substrate to ensure that the substrate is completely dispersed in the anhydrous ethanol, add 0.5 mL of ethyl silicate per gram of substrate, add 0.1 mL of acetic acid per gram of substrate and mix well, immerse for 60 min, and treat for 48 h at -60 °C and a vacuum degree of less than 0.1 mbar to obtain an adsorbent.

[0127] The adsorbent prepared in this example was subjected to the same characterization and performance testing as in Example 1, and the results are as follows.

[0128] Porosity (%) Permeability (m2) Adsorption rate g / (g·min) Saturated moisture absorption (g / g) Regeneration efficiency (%) 91.7 10-14 0.0207 1.470 87

[0129] The affinity of the adsorbent in this example to water molecules is not as good as that of the adsorbent in Example 2. The electronic interaction between the biomass hydroxyl group and the ester group of the organic protective layer is weak, resulting in poor stability of the adsorbent. At the same time, after contacting water molecules, the inorganic salt hydrate has a high degree of crystallinity and a more serious pore blocking effect, which seriously affects the adsorption effect.

[0130] The same pressurized saturated moisture absorption experiment was carried out. The results showed that the initial adsorption rate under the pressurized saturated moisture absorption experiment was about 0.0146 g / (g·min), the initial saturated moisture absorption was 1.221 g / g adsorbent, and the regeneration efficiency reached 74%. The high-pressure cycle resistance of the adsorbent prepared in this example is relatively weak, because in the continuous adsorption process, the inorganic salt hydrate continuously blocks the pores, which not only leads to a significant decrease in the adsorption rate and moisture absorption, but also leads to continuous collapse of the pore structure, and the adsorbent itself is continuously damaged.

[0131] Comparative Example 5

[0132] A method for preparing an adsorbent, the method comprising:

[0133] 1) 5 g of sodium sulfite, 11 g of sodium hydroxide and 100 mL of water were mixed evenly to obtain an alkali solution, 10 g of microcrystalline cellulose was added and mixed evenly, and the mixture was kept at 80 °C for 6 h. After filtering and drying, the solid product was obtained. 50 mL of anhydrous ethanol, 13 g of aluminum chloride and 1.3 g of magnesium chloride were added and mixed evenly, and the solid product was taken out after filtering and drying. The solid product was pyrolyzed in a nitrogen atmosphere at 350 °C for 10 min to obtain a pyrolysis product;

[0134] 2) adding the pyrolysis product to a 24 wt% lithium chloride aqueous solution, the amount of which is 3 mL / g of the pyrolysis product, mixing and stirring the reaction for 8 h, filtering, washing, and drying, and then adding the solution to a 10 wt% calcium chloride aqueous solution, the amount of which is 3 mL / g of the pyrolysis product, mixing and stirring the reaction for 8 h to obtain an intermediate product, placing the intermediate product at 900 ° C, keeping the temperature constant for 2.5 h, immersing the material in 2 mol / L hydrochloric acid at 100 ° C, treating for 12 h, filtering, washing, and drying to obtain a substrate;

[0135] 3) Add 25 mL of anhydrous ethanol per gram of substrate to ensure that the substrate is completely dispersed in the anhydrous ethanol, add 0.5 mL of ethyl silicate per gram of substrate, add 0.1 mL of acetic acid per gram of substrate and mix well, immerse for 60 min, and treat for 48 h at -60 °C and a vacuum degree of less than 0.1 mbar to obtain an adsorbent.

[0136] The adsorbent prepared in this example was subjected to the same characterization and performance testing as in Example 1, and the results are as follows.

[0137] Porosity (%) Permeability (m2) Adsorption rate g / (g·min) Saturated moisture absorption (g / g) Regeneration efficiency (%) 91.8 10-14 0.0184 1.549 89

[0138] Too low a calcination temperature results in the formation of η-Al2O3, but no γ-Al2O3. The static capacity of another low-temperature phase alumina η-Al2O3 is low, which significantly affects the adsorption of the adsorbent. Although η-Al2O3 has the characteristics of large pore volume, it is difficult to produce a stable and effective adsorption effect. The large pore volume also makes the hygroscopic carrier in its pores easily damaged, resulting in a significant decrease in regeneration efficiency after multiple cycles.

[0139] The same pressurized saturated moisture absorption experiment was carried out. The results showed that the initial adsorption rate under the conditions of the pressurized saturated moisture absorption experiment was about 0.0182 g / (g·min), the initial saturated moisture absorption capacity was 1.466 g / g adsorbent, and the regeneration efficiency reached 86%. Although there are not many studies on η-Al2O3 as a water adsorbent / desiccant, it can be seen to a certain extent in this case that η-Al2O3 alumina has a weaker direct performance than γ-Al2O3 alumina, but it seems to have certain advantages in high pressure resistance. Perhaps in the subsequent research process, strengthening its own adsorption rate, moisture absorption capacity and regeneration efficiency based on this feature will produce a new type of alumina desiccant that is more suitable for high-pressure gas drying.

[0140] Comparative Example 6

[0141] A method for preparing an adsorbent, the method comprising:

[0142] 1) 5 g of sodium sulfite, 11 g of sodium hydroxide and 100 mL of water were mixed evenly to obtain an alkali solution, 10 g of microcrystalline cellulose was added and mixed evenly, and the mixture was kept at 80 °C for 6 h. After filtering and drying, the solid product was obtained. 50 mL of anhydrous ethanol, 13 g of aluminum chloride and 1.3 g of magnesium chloride were added and mixed evenly, and the solid product was taken out after filtering and drying. The solid product was pyrolyzed in a nitrogen atmosphere at 350 °C for 10 min to obtain a pyrolysis product;

[0143] 2) The pyrolysis product was added to a 24 wt% lithium chloride aqueous solution, the amount of which was 3 mL / g of the pyrolysis product, and the mixture was stirred for 8 h. After filtering, washing, and drying, the mixture was added to a 10 wt% calcium chloride aqueous solution, the amount of which was 3 mL / g of the pyrolysis product, and the mixture was stirred for 8 h to obtain an intermediate product. The intermediate product was placed at 550 °C and kept at a constant temperature for 2.5 h. The material was immersed in 2 mol / L hydrochloric acid at 100 °C for 12 h. The adsorbent was filtered, washed, and dried to obtain the adsorbent.

[0144] The adsorbent prepared in this example was subjected to the same characterization and performance testing as in Example 1, and the results are as follows.

[0145] Porosity (%) Permeability (m2) Adsorption rate g / (g·min) Saturated moisture absorption (g / g) Regeneration efficiency (%) 92.8 10-14 0.0175 1.439 84

[0146] The capillary structure of the adsorbent in this example is simple and lacks the protection of ethyl silicate. The active sites of the secondary structure of aluminum oxide are easily lost in a high temperature environment. Compared with Example 2, its adsorption effect is significantly reduced.

[0147] Comparative Example 7

[0148] A commercially available activated alumina adsorbent (water desiccant) was used.

[0149] The adsorbents in Example 2 and this example were tested for cycles. The results showed that the equilibrium adsorption capacity of commercially available adsorbents was significantly reduced with the increase in the number of cycles. In a long-term hot and humid environment, the commercially available adsorbent skeleton collapsed, and the pores slowly decreased with the cycle, which obviously reduced the adsorption capacity of water molecules. The saturated adsorption experiments under normal pressure (1.0±0.05 atm) and supercharged pressure (12.0±0.2 atm) showed limited performance. Under normal pressure, it showed an initial adsorption rate of about 0.0106 g / (g·min), an initial saturated moisture absorption of 0.471 g / g adsorbent, and a regeneration efficiency of 73%. Under supercharging, it showed an initial adsorption rate of about 0.0079 g / (g·min), an initial saturated moisture absorption of 0.218 g / g adsorbent, and a regeneration efficiency of 51%. It can be seen that conventional commercially available activated alumina adsorbents do not have good regeneration, especially under high pressure conditions, and their performance will drop rapidly after multiple cycles.

[0150] Application Examples

[0151] Take the adsorbents prepared in Examples 1 to 3 above, and place them in an environment with a relative humidity of 10% and 30% for dehumidification for 24 h, respectively. The environment is a closed environment and the pressure of the compressed air is 12.0±0.2 atm. The amount of adsorbent is 50 g / m3 of the compressed air volume in the environment. A complete drying test is carried out, and the results are as follows (average values ​​are taken).

[0152]

[0153] The complete drying time is the time when the dew point temperature of the experimental environment reaches -51.75 ℃.

[0154] In an environment with a relative humidity of 10%, water molecules fill the micropores of the adsorbent, and the amount of adsorption depends on the richness of the capillary structure of the adsorbent, and the dehumidification effect is as high as 99.9% or more. In an environment with a relative humidity of 30%, water molecules will hydrogen bond with water molecules around the adsorption sites in the pores to further form water molecule clusters. At this time, the sufficient space provided by the adsorbent enables it to have an excellent saturated adsorption capacity. At the same time, the capillary structure and hydrophilic adsorption sites enable the adsorbent to have a long-term dehumidification ability, and the dehumidification effect can also exceed 99.9%, indicating that the adsorbent of the present invention exhibits excellent performance in both high and low humidity environments. At the same time, with the increase of relative humidity, the adsorption rate also shows a relative increase, and the comparison with the aforementioned Examples 1 to 3 can also confirm this phenomenon.

Claims

1. A method for preparing an adsorbent, characterized in that: The method comprises: 1) Mix the polysaccharide raw material and alkali solution evenly, heat, filter and dry, then add the solvent, aluminum salt and magnesium salt and mix evenly, filter and dry, perform pyrolysis pretreatment and obtain pyrolysis products; 2) adding the pyrolysis product to a lithium salt solution for a mixed reaction, filtering, washing, and drying, and then adding it to a calcium salt solution for a mixed reaction to obtain an intermediate product, and sequentially subjecting the intermediate product to a high temperature treatment, an acid solution immersion treatment, filtering, washing, and drying to obtain a substrate; 3) Dispersing the substrate in a solvent, adding inorganic acid ester and acid solution, mixing evenly, and freeze-drying to obtain an adsorbent; Step 1) the polysaccharide raw material is microcrystalline cellulose; Step 1) The pyrolysis pretreatment is carried out at 300-350°C for 10-15 minutes; Step 2) The high temperature treatment is carried out at 550-600°C for 2-2.5 hours; Step 3) The inorganic acid ester is ethyl silicate.

2. The method for preparing an adsorbent according to claim 1, characterized in that: Step 1) The dosage of the alkali solution is 10-15 mL / g polysaccharide raw material, and the preparation method is as follows: Take sodium sulfite and sodium hydroxide in a mass ratio of 1: (2-2.2), add 15-25 mL of water per gram of sodium sulfite and mix well; In step 1), the heating is carried out at 80-90°C and kept at a constant temperature for 5-6 hours.

3. The method for preparing an adsorbent according to claim 1 or 2, characterized in that: Step 1) the solvent is anhydrous ethanol, and the amount thereof is 5-10 mL / g polysaccharide raw material; Step 1) the aluminum salt is aluminum chloride, and its usage is 1.3-1.6 g / g polysaccharide raw material; Step 1) The magnesium salt is magnesium chloride, and its dosage is 0.1-0.15 g / g polysaccharide raw material.

4. The method for preparing an adsorbent according to claim 1, characterized in that: Step 2) the lithium salt solution is a lithium chloride aqueous solution with a concentration of 22 to 28 wt % and an amount of 3 to 5 mL / g of pyrolysis product; The reaction time of adding the mixture into the lithium salt solution for the mixed reaction is 6 to 12 hours.

5. The method for preparing an adsorbent according to claim 1, characterized in that: Step 2) the calcium salt solution is a calcium chloride aqueous solution with a concentration of 7 to 13 wt % and an amount of 3 to 5 mL / g of pyrolysis product; The reaction time of adding to the calcium salt solution for mixed reaction is 6 to 12 hours.

6. The method for preparing an adsorbent according to claim 1, 4 or 5, characterized in that: In step 2), the acid immersion treatment is carried out at 100°C, using hydrochloric acid with a concentration of 1 to 2 mol / L to immerse the intermediate product for a treatment time of 12 to 14 hours.

7. The method for preparing an adsorbent according to claim 1, characterized in that: Step 3) The solvent is anhydrous ethanol, and 25 to 30 mL of the solvent is added per gram of substrate; Step 3) the inorganic acid ester is used at a ratio of 0.5 to 0.8 mL per gram of substrate; Step 3) the acid solution is acetic acid, and 0.1 to 0.2 mL of the acid solution is added per gram of substrate; Step 3) The immersion treatment time is 30 to 60 minutes.

8. The method for preparing an adsorbent according to claim 1 or 7, characterized in that: Step 3) The freeze drying is carried out at -60 to -50°C and a vacuum degree of less than 0.1 mbar for 48 to 52 hours.

9. An adsorbent prepared by the method of any one of claims 1 to 8, characterized in that: The adsorbent is an alumina-based adsorbent, and the alumina forms a hollow structure oxide.

10. A use of the adsorbent as claimed in claim 9, characterized in that: The adsorbent is used to dry compressed gas.