A lithium-rich manganese-based precursor, positive electrode material, preparation method and application thereof
A two-step precipitation reaction with nickel, manganese, aluminum, and titanium salts forms a lithium-rich manganese-based precursor, addressing manganese agglomeration and lithium volatilization issues, resulting in improved lithium-ion battery performance.
Patent Information
- Application Number
- CN202411075405.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-07
AI Technical Summary
Existing technologies face challenges in preparing cobalt-free single-crystal lithium-rich manganese-based materials due to manganese agglomeration and low lithium insertion rates, which affect the performance of lithium-ion battery cathode materials.
A method involving a two-step precipitation reaction using mixed salt solutions of nickel, manganese, aluminum, and titanium salts, followed by sintering with lithium salts, to form a lithium-rich manganese-based precursor with in-situ doping of Ti and Al ions, refining particle size and preventing manganese agglomeration.
The method results in a lithium-rich manganese-based positive electrode material with improved performance by increasing the specific surface area, enhancing particle fusion, and preventing lithium volatilization, leading to better energy density and safety in lithium-ion batteries.
Smart Images

Figure CN118598218B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of lithium-ion batteries, and in particular to a lithium-rich manganese-based precursor, a positive electrode material, and a preparation method and application thereof. Background Art
[0002] Lithium batteries are gradually being used in all aspects of human life due to their light weight, high energy density, and pollution-free characteristics. At present, the cathode materials of lithium-ion batteries mainly include lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, and ternary materials. Traditional ternary materials have good cycle stability and high capacity, but they still cannot meet the future demand for power batteries for electric vehicles. Therefore, it has become an urgent need to develop and improve the energy density of lithium-ion battery cathode materials, while improving safety and reducing battery costs.
[0003] Lithium-rich manganese-based positive electrode materials have attracted more and more attention due to their low price, environmental friendliness, and higher specific capacity than ternary materials. However, it is difficult to prepare cobalt-free single-crystal lithium-rich manganese-based materials with the existing technology, and the prepared cobalt-free lithium-rich manganese-based single-crystal materials are prone to manganese agglomeration. In view of this, the present invention provides a lithium-rich manganese-based precursor, a positive electrode material, and a preparation method and application. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a lithium-rich manganese-based precursor, a positive electrode material, and a preparation method and application thereof, with the purpose of improving the performance of the lithium-rich manganese-based positive electrode material.
[0005] The technical solution of the present invention to solve the above technical problems is as follows:
[0006] In a first aspect, a method for preparing a lithium-rich manganese-based precursor comprises the following steps: subjecting a first mixed salt solution to a precipitation reaction to form a core of a lithium-rich manganese-based precursor, and then adding a second mixed salt solution (to the first mixed salt solution after the previous precipitation reaction), and continuing the precipitation reaction to form a lithium-rich manganese-based precursor; the first mixed salt comprises a nickel salt and a manganese salt; and the second mixed salt comprises an aluminum salt and a titanium salt.
[0007] The beneficial effects of the present invention are as follows: the first mixed salt solution first forms the core of the lithium-rich manganese-based precursor through a precipitation reaction and then slowly introduces the second mixed salt solution to achieve in-situ doping of Ti ions and Al ions, thereby refining the particle size of the precursor, making the surface area of the lithium-rich manganese-based precursor larger, and increasing the contact area with the lithium salt after mixing with the lithium salt, which is conducive to the mutual fusion between the particles; and by in-situ doping of Ti ions and Al ions, fast ion conductors lithium titanate and lithium aluminate can appear in low-temperature local areas during the sintering process of the lithium-rich manganese-based precursor to form a positive electrode material, and at the same time, the problem of more serious volatilization of lithium salts under high temperature conditions can be avoided, and the problem of manganese agglomeration caused by the formation of Li2MnO3 at low temperature to reduce the lithium insertion rate can be compensated, thereby making the prepared lithium-rich manganese-based positive electrode material have better performance.
[0008] Based on the above technical solution, the present invention can also be improved as follows.
[0009] Further, the particle size D50 of the core of the lithium-rich manganese-based precursor is 0.8 μm to 1.2 μm; the particle size D50 of the lithium-rich manganese-based precursor is 3 μm to 5 μm;
[0010] And / or, the nickel salt includes at least one of nickel sulfate and nickel nitrate;
[0011] And / or, the manganese salt includes at least one of manganese sulfate and manganese nitrate;
[0012] And / or, the aluminum salt includes at least one of aluminum sulfate and aluminum nitrate;
[0013] And / or, the titanium salt includes at least one of TiOSO4, Ti2O3(SO4), and Ti4O5(SO4)3.
[0014] The beneficial effect of adopting the above-mentioned further scheme is: the first mixed salt solution of the present invention first forms the core of the lithium-rich manganese-based precursor through a precipitation reaction and then slowly introduces the second mixed salt solution, and the specific surface area of the prepared lithium-rich manganese-based precursor is further increased through the hydrolysis reaction of TiOSO4, and / or Ti2O3(SO4), and / or Ti4O5(SO4)3, thereby avoiding the use of a one-time preparation of a mixed solution containing nickel salt, manganese salt, titanium salt and aluminum salt to form a lithium-rich manganese-based precursor through a precipitation reaction, which results in the lithium-rich manganese-based precursor not being prepared yet, and the titanium salt has been completely hydrolyzed, and the effect of further refining the primary particles of the precursor cannot be achieved.
[0015] Furthermore, the molar ratio of the nickel element in the nickel salt to the manganese element in the manganese salt is 25:75~40:60; the aluminum element in the aluminum salt accounts for 0.4%~0.6% of the total amount of the nickel element in the nickel salt and the manganese element in the manganese salt; the titanium element in the titanium salt accounts for 0.1%~0.3% of the total amount of the nickel element in the nickel salt and the manganese element in the manganese salt.
[0016] The beneficial effect of adopting the above further scheme is that by adopting the above dosage, the specific surface area of the prepared lithium-rich manganese-based precursor is larger, and the dosage of in-situ doping of Ti ions and Al ions is more precise.
[0017] Further, the method comprises the following specific steps: adding a precipitant and a complexing agent to a first mixed salt solution to carry out a precipitation reaction to form a core of a lithium-rich manganese-based precursor, then adding a second mixed salt solution, a precipitant and a complexing agent to continue a precipitation reaction to form a lithium-rich manganese-based precursor, and then aging, washing and drying in sequence to obtain a lithium-rich manganese-based precursor;
[0018] The precipitant includes at least one of sodium hydroxide and potassium hydroxide; the complexing agent includes at least one of ammonia water and ammonium sulfate;
[0019] The concentration of the complexing agent is 5 mol / L to 15 mol / L.
[0020] The beneficial effect of adopting the above further scheme is: using a high complexing agent concentration can further refine the particle size of the precursor, forming a lithium-rich manganese-based precursor with a large specific surface area and small secondary spheres, which increases the contact area with the lithium salt after mixing with the lithium salt, which is conducive to the fusion between the particles.
[0021] Furthermore, the parameters of the precipitation reaction are: reaction temperature of 45°C to 55°C, stirring speed of 400rpm to 900rpm, and pH of 10.8 to 11.2.
[0022] The beneficial effect of adopting the above further scheme is that the present invention adopts a higher rotation speed and a higher reaction temperature to further refine the particle size of the precursor, forming a precursor with a larger specific surface area and smaller secondary spheres.
[0023] In a second aspect, a lithium-rich manganese-based precursor is provided, wherein the lithium-rich manganese-based precursor is prepared by the preparation method.
[0024] The beneficial effects of adopting the above scheme are: the lithium-rich manganese-based precursor has a larger surface area, and the contact area with the lithium salt is increased after mixing with the lithium salt, which is conducive to the mutual fusion of particles; and through the doped Ti ions and Al ions, fast ion conductors lithium titanate and lithium aluminate can appear in low-temperature local areas during the sintering process of the lithium-rich manganese-based precursor to form a positive electrode material. At the same time, the problem of more serious volatilization of lithium salts under high temperature conditions can be avoided, and the problem of manganese agglomeration caused by the formation of Li2MnO3 at low temperature to reduce the lithium insertion rate can be compensated, thereby making the performance of the lithium-rich manganese-based positive electrode material more excellent.
[0025] In a third aspect, a lithium-rich manganese-based positive electrode material is provided, wherein the lithium-rich manganese-based positive electrode material is prepared from the lithium-rich manganese-based precursor prepared by the preparation method or the lithium-rich manganese-based precursor.
[0026] The beneficial effect of adopting the above scheme is that the lithium-rich manganese-based positive electrode material of the present invention has better performance.
[0027] In a fourth aspect, a method for preparing a lithium-rich manganese-based positive electrode material comprises the following steps: mixing the lithium-rich manganese-based precursor obtained by the preparation method or the lithium-rich manganese-based precursor with a lithium salt and sintering them to obtain a lithium-rich manganese-based positive electrode material.
[0028] The beneficial effect of adopting the above scheme is that by adopting the above lithium-rich manganese-based precursor, the prepared lithium-rich manganese-based positive electrode material has better performance and a simple process.
[0029] Furthermore, the ratio of the total amount of nickel and manganese in the lithium-rich manganese-based precursor to the amount of lithium in the lithium salt is 1:1.2-1.45;
[0030] The lithium salt includes at least one of lithium hydroxide, lithium carbonate, lithium oxide and lithium chloride;
[0031] The sintering parameters are as follows: sintering temperature is 850° C. to 1000° C., sintering time is 8 h to 18 h, sintering atmosphere is oxygen, and sintering heating and cooling rates are 1° C. / min to 10° C. / min.
[0032] The beneficial effect of adopting the above further scheme is: a single crystal lithium-rich manganese-based positive electrode material with better particle dispersion is formed through the above scheme.
[0033] A fifth aspect provides a lithium-ion battery, comprising the lithium-rich manganese-based positive electrode material.
[0034] The beneficial effect of adopting the above scheme is that the performance of the lithium-ion battery is more excellent due to the inclusion of the lithium-rich manganese-based positive electrode material of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1This is a SEM image of the lithium-rich manganese-based positive electrode material prepared in Example 1 of the present invention;
[0036] Figure 2 This is a diagram of a Ti-doped lithium-rich manganese-based positive electrode material prepared in Comparative Example 1 of the present invention;
[0037] Figure 3 This is a diagram of an Al-doped lithium-rich manganese-based positive electrode material prepared in Comparative Example 2 of the present invention;
[0038] Figure 4 This is a diagram of the undoped lithium-rich manganese-based positive electrode material prepared in Comparative Example 3 of the present invention. DETAILED DESCRIPTION
[0039] The principles and features of the present invention are described below, and the examples are only used to explain the present invention and are not used to limit the scope of the present invention. If no specific technology or conditions are specified in the embodiments, the technology or conditions described in the literature in this field or the product instructions are used. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased through regular channels.
[0040] The present embodiment relates to a method for preparing a lithium-rich manganese-based precursor, comprising the following steps: subjecting a first mixed salt solution to a precipitation reaction to form the core of a lithium-rich manganese-based precursor, and then continuously adding a second mixed salt solution in small amounts (to the first mixed salt solution after the previous precipitation reaction), and continuing the precipitation reaction to form a lithium-rich manganese-based precursor; the first mixed salt comprises a nickel salt and a manganese salt; the second mixed salt comprises an aluminum salt and a titanium salt.
[0041] The pH value of the lithium-rich manganese-based precursor formed by adding the second mixed salt solution to react is 10.8-11.2, and the ammonia content is 0.8-1.2 g / L. For example, the corresponding flow rate ratio of the second mixed salt solution to the first mixed salt solution is 1:1.
[0042] In this embodiment, the particle size D50 of the core of the lithium-rich manganese-based precursor is preferably 0.8 μm to 1.2 μm, specifically 0.8 μm, 0.9 μm, 1.0 μm, 1.1 μm, 1.2 μm, etc.; the particle size D50 of the lithium-rich manganese-based precursor is 3 μm to 5 μm, specifically 3 μm, 4 μm, 5 μm, etc.;
[0043] And / or, the nickel salt includes at least one of nickel sulfate and nickel nitrate;
[0044] And / or, the manganese salt includes at least one of manganese sulfate and manganese nitrate;
[0045] And / or, the aluminum salt includes at least one of aluminum sulfate and aluminum nitrate;
[0046] And / or, the titanium salt includes at least one of TiOSO4, Ti2O3(SO4), and Ti4O5(SO4)3.
[0047] In this embodiment, the molar ratio of the nickel element in the nickel salt to the manganese element in the manganese salt is 25:75~40:60, specifically 25:75, 33:67, 40:60, etc.; the aluminum element in the aluminum salt accounts for 0.4%~0.6% of the total amount of the nickel element in the nickel salt and the manganese element in the manganese salt, specifically 0.4%, 0.45%, 0.5%, 0.6%, etc.; the titanium element in the titanium salt accounts for 0.1%~0.3% of the total amount of the nickel element in the nickel salt and the manganese element in the manganese salt, specifically 0.1%, 0.15%, 0.2%, 0.3%, etc.;
[0048] The concentration of each salt in the first mixed salt solution is 1 mol / L to 3 mol / L, specifically 1 mol / L, 2 mol / L, 3 mol / L, etc.
[0049] The present embodiment preferably includes the following specific steps: adding a precipitant and a complexing agent to a first mixed salt solution to carry out a precipitation reaction to form a core of a lithium-rich manganese-based precursor, then adding a second mixed salt solution, a precipitant and a complexing agent to continue a precipitation reaction to form a lithium-rich manganese-based precursor, and then aging, washing and drying in sequence to obtain a lithium-rich manganese-based precursor;
[0050] The above-mentioned aging, washing and drying are specific: the aging treatment temperature is 40°C, the time is 1h~4h, specifically 1h, 2h, 3h, 4h, etc.; after the aging is completed, it is washed alternately with a 75°C alkaline solution and pure water; then the filter cake is placed in a 120°C blast oven for 2h~5h, specifically 2h, 3h, 4h, 5h, etc., and then passed through a 300-mesh sieve to obtain a powdered product, that is, a lithium-rich manganese-based precursor;
[0051] The precipitant includes at least one of sodium hydroxide and potassium hydroxide; the complexing agent includes at least one of ammonia water and ammonium sulfate;
[0052] The concentration of the complexing agent is 5 mol / L to 15 mol / L, specifically 5 mol / L, 10 mol / L, 15 mol / L and the like.
[0053] In this embodiment, the parameters of the precipitation reaction are as follows: the reaction temperature is 45°C~55°C, specifically 45°C, 50°C, 55°C, etc., the stirring speed is 400rpm~900rpm, specifically 400rpm, 600rpm, 800rpm, 900rpm, etc., and the pH is 10.8~11.2, specifically 10.8, 11, 11.2, etc.
[0054] This embodiment also relates to a lithium-rich manganese-based precursor, and the lithium-rich manganese-based precursor is prepared by the preparation method.
[0055] The present embodiment also relates to a lithium-rich manganese-based positive electrode material, wherein the lithium-rich manganese-based positive electrode material is prepared from the lithium-rich manganese-based precursor prepared by the preparation method or the lithium-rich manganese-based precursor.
[0056] The present embodiment also relates to a method for preparing a lithium-rich manganese-based positive electrode material, comprising the following steps: mixing the lithium-rich manganese-based precursor obtained by the preparation method or the lithium-rich manganese-based precursor with a lithium salt and sintering them to obtain a lithium-rich manganese-based positive electrode material.
[0057] In this embodiment, preferably, the ratio of the total amount of nickel and manganese in the lithium-rich manganese-based precursor to the amount of lithium in the lithium salt is 1:1.2-1.45, specifically 1:1.2, 1:1.25, 1:1.3, 1:1.45, etc.;
[0058] The lithium salt includes at least one of lithium hydroxide, lithium carbonate, lithium oxide and lithium chloride;
[0059] The sintering parameters are as follows: sintering temperature is 850℃~1000℃, specifically 850℃, 900℃, 950℃, 1000℃, etc., sintering time is 8h~18h, specifically 8h, 10h, 15h, 18h, etc., sintering atmosphere is oxygen, and sintering heating and cooling rates are 1℃ / min~10℃ / min, specifically 1℃ / min, 5℃ / min, 10℃ / min, etc.
[0060] This embodiment also relates to a lithium-ion battery, which includes the lithium-rich manganese-based positive electrode material.
[0061] In summary, the present invention adopts a higher rotation speed, a high ammonia concentration, a higher reaction temperature and in-situ doping of Ti and Al to achieve the purpose of refining the particles of the lithium-rich manganese-based precursor, so that it forms a precursor with a larger specific surface area and smaller secondary spheres. After mixing with the lithium salt, the contact area with the lithium salt is increased, which is conducive to the mutual fusion between the particles; and by in-situ doping of Ti ions and Al ions, during the sintering process of the lithium-rich manganese-based precursor to form the positive electrode material, fast ion conductors lithium titanate and lithium aluminate can appear in the low-temperature local area, and at the same time, the problem of more serious volatilization of lithium salts under high temperature conditions can be avoided, which makes up for the problem of manganese agglomeration caused by the formation of Li2MnO3 at low temperature to reduce the lithium insertion rate, thereby making the prepared lithium-rich manganese-based positive electrode material have better performance. The cobalt-free single crystal lithium-rich manganese-based positive electrode material prepared by the present invention has a compaction density increased to 3.20g / cm 3 The following is a detailed description through specific examples and comparative examples.
[0062] Example 1
[0063] This embodiment relates to a method for preparing a lithium-rich manganese-based positive electrode material, comprising the following steps:
[0064] (1) According to the molar ratio of Ni:Mn=33:67, NiSO4·6H2O and MnSO4·H2O were weighed and dissolved in deionized water to prepare a 2 mol / L first mixed salt solution; at the same time, titanium oxysulfate and aluminum sulfate were weighed and dissolved in 600 ml deionized water according to the total amount of Ni and Mn elements of 0.2% and 0.5% respectively to prepare a second mixed salt solution, and at the same time, 5 mol / L sodium hydroxide solution was prepared as a precipitant and 10 mol / L ammonia water was prepared as a complexing agent; deionized water was added to a 6 L reactor to cover the upper stirring paddle, the stirring speed was set to 700 rpm and kept on, and then ammonia water and sodium hydroxide solution were added to adjust the pH value of the deionized water so that the pH value of the deionized water in the reactor was adjusted to 11.0 and the ammonia content was 1.0 g / L;
[0065] (2) The first mixed salt solution, sodium hydroxide solution and ammonia water prepared above are added into the reactor by a metering pump. The temperature of the reactor is controlled at 50°C, and a small amount of the second mixed salt solution is continuously introduced during the reaction (the flow rate ratio with the mixed salt solution is 1:1). During the reaction, the pH value in the reactor is adjusted by the inlet flow rate of the sodium hydroxide solution according to the growth of the particle size, so that its average value is maintained at 10.8-11.2. As the inlet time increases, the particles generated by the reaction gradually grow and the crystallinity is continuously improved. After the precursor forms a nucleus (the median particle size D50 of the precursor reaches 0.8μm~1.2μm), the second mixed salt solution is continuously introduced in small amounts (the flow rate ratio with the first mixed salt solution is 1:1). During the reaction, the slurry particle size is tested with a laser particle size analyzer every 2 hours. By adjusting the pH value in the reactor, the median particle size D50 of the precursor is 3μm~5μm; the overflow material with qualified particle size is collected and the overflow material flows into the aging device for aging treatment (temperature is 40℃, time is 1h~4h). After aging, it is washed alternately with 75℃ alkaline solution and pure water. Then the filter cake is placed in a 120℃ blast oven for 2h~5h, and then passed through a 300-mesh sieve to obtain a powdered product, i.e., a cobalt-free single crystal manganese-rich precursor material.
[0066] (3) The obtained cobalt-free single crystal manganese-rich precursor material and lithium hydroxide are mixed at a molar ratio of Li: (Ni + Mn) = 1.3:1, and after the qualified mixture is placed in a sagger, transferred into a furnace body for sintering, the sintering temperature is 900°C, the sintering atmosphere is oxygen, and the sintering heating and cooling rates are 5°C / min. After the sintering is completed, a cobalt-free single crystal lithium-rich manganese-based positive electrode material is obtained.
[0067] Powder resistivity test: pressure range: 0~200MPa; 0~50MPa, interval 10MPa, 50MPa~200MPa, interval 50MPa, pressure holding 10s; measured compaction density 3.2g / cm 3 .
[0068] Example 2
[0069] (1) According to the molar ratio of Ni:Mn=25:75, NiSO4·6H2O and MnSO4·H2O were weighed and dissolved in deionized water to prepare a 2 mol / L first mixed salt solution; at the same time, titanium oxysulfate and aluminum sulfate were weighed and dissolved in 600 ml deionized water according to the total amount of Ni and Mn elements of 0.1% and 0.4% respectively to prepare a second mixed salt solution, and at the same time, 5 mol / L sodium hydroxide solution was prepared as a precipitant and 10 mol / L ammonia water was prepared as a complexing agent; deionized water was added to a 6 L reactor to cover the upper stirring paddle, the stirring speed was set to 300 rpm and kept on, and then ammonia water and sodium hydroxide solution were added to adjust the pH value of the deionized water so that the pH value of the deionized water in the reactor was adjusted to 11.0 and the ammonia content was 1.0 g / L;
[0070] (2) The first mixed salt solution, sodium hydroxide solution and ammonia water prepared above are added into the reactor by a metering pump. The temperature of the reactor is controlled at 50°C, and a small amount of the second mixed salt solution is continuously introduced during the reaction (the flow rate ratio with the mixed salt solution is 1:1). During the reaction, the pH value in the reactor is adjusted by the inlet flow rate of the sodium hydroxide solution according to the growth of the particle size, so that its average value is maintained at 10.8-11.2. As the inlet time increases, the particles generated by the reaction gradually grow and the crystallinity is continuously improved. After the precursor forms a nucleus (the median particle size D50 of the precursor reaches 0.8μm~1.2μm), the second mixed salt solution is continuously introduced in small amounts (the flow rate ratio with the first mixed salt solution is 1:1). During the reaction, the slurry particle size is tested with a laser particle size analyzer every 2 hours. By adjusting the pH value in the reactor, the median particle size D50 of the precursor is 3μm~5μm; the overflow material with qualified particle size is collected and the overflow material flows into the aging device for aging treatment (temperature is 40℃, time is 1h~4h). After aging, it is washed alternately with 75℃ alkaline solution and pure water. Then the filter cake is placed in a 120℃ blast oven for 2h~5h, and then passed through a 300-mesh sieve to obtain a powdered product, i.e., a cobalt-free single crystal manganese-rich precursor material.
[0071] (3) The obtained cobalt-free single crystal manganese-rich precursor material and lithium hydroxide are mixed at a molar ratio of Li: (Ni + Mn) = 1.2:1, and after the qualified mixture is placed in a sagger, transferred into a furnace body for sintering, the sintering temperature is 850°C, the sintering atmosphere is oxygen, and the sintering heating and cooling rates are 1°C / min. After the sintering is completed, a cobalt-free single crystal lithium-rich manganese-based positive electrode material is obtained.
[0072] Powder resistivity test: pressure range: 0~200MPa; 0~50MPa, interval 10MPa, 50MPa~200MPa, interval 50MPa, pressure holding 10s; measured compaction density 2.78g / cm 3 .
[0073] Example 3
[0074] (1) According to the molar ratio of Ni:Mn=40:60, NiSO4·6H2O and MnSO4·H2O were weighed and dissolved in deionized water to prepare a 2 mol / L first mixed salt solution; at the same time, titanium oxysulfate and aluminum sulfate were weighed and dissolved in 600 ml deionized water according to the total amount of Ni and Mn elements of 0.3% and 0.6% respectively to prepare a second mixed salt solution, and at the same time, 5 mol / L sodium hydroxide solution was prepared as a precipitant and 10 mol / L ammonia water was prepared as a complexing agent; deionized water was added to a 6 L reactor to cover the upper stirring paddle, the stirring speed was set to 1000 rpm and kept on, and then ammonia water and sodium hydroxide solution were added to adjust the pH value of the deionized water so that the pH value of the deionized water in the reactor was adjusted to 11.0 and the ammonia content was 1.0 g / L;
[0075] (2) The first mixed salt solution, sodium hydroxide solution and ammonia water prepared above are added into the reactor by a metering pump. The temperature of the reactor is controlled at 50°C, and a small amount of the second mixed salt solution is continuously introduced during the reaction (the flow rate ratio with the mixed salt solution is 1:1). During the reaction, the pH value in the reactor is adjusted by the inlet flow rate of the sodium hydroxide solution according to the growth of the particle size, so that its average value is maintained at 10.8-11.2. As the inlet time increases, the particles generated by the reaction gradually grow and the crystallinity is continuously improved. After the precursor forms a nucleus (the median particle size D50 of the precursor reaches 0.8μm~1.2μm), the second mixed salt solution is continuously introduced in small amounts (the flow rate ratio with the first mixed salt solution is 1:1). During the reaction, the slurry particle size is tested with a laser particle size analyzer every 2 hours. By adjusting the pH value in the reactor, the median particle size D50 of the precursor is 3μm~5μm; the overflow material with qualified particle size is collected and the overflow material flows into the aging device for aging treatment (temperature is 40℃, time is 1h~4h). After aging, it is washed alternately with 75℃ alkaline solution and pure water. Then the filter cake is placed in a 120℃ blast oven for 2h~5h, and then passed through a 300-mesh sieve to obtain a powdered product, i.e., a cobalt-free single crystal manganese-rich precursor material.
[0076] (3) The obtained cobalt-free single crystal manganese-rich precursor material and lithium hydroxide are mixed at a molar ratio of Li: (Ni + Mn) = 1.45:1, and after the qualified mixture is placed in a sagger, transferred into a furnace body for sintering, the sintering temperature is 1000°C, the sintering atmosphere is oxygen, and the sintering heating and cooling rates are both 10°C / min. After the sintering is completed, a cobalt-free single crystal lithium-rich manganese-based positive electrode material is obtained.
[0077] Powder resistivity test: pressure range: 0~200MPa; 0~50MPa, interval 10MPa, 50MPa~200MPa, interval 50MPa, pressure holding 10s; measured compaction density 2.72g / cm 3 .
[0078] Comparative Example 1
[0079] This comparative example relates to a method for preparing a Ti-doped lithium-rich manganese-based positive electrode material, comprising the following steps:
[0080] (1) According to the molar ratio of Ni:Mn=33:67, NiSO4·6H2O and MnSO4·H2O were weighed and dissolved in deionized water to prepare a 2 mol / L first mixed salt solution; at the same time, titanyl sulfate was weighed according to 0.2% of the total amount of Ni and Mn elements and dissolved in 600 ml of deionized water to prepare a titanyl sulfate solution, and 5 mol / L sodium hydroxide solution was prepared as a precipitant and 10 mol / L ammonia water as a complexing agent; deionized water was added to a 6 L reactor to cover the upper stirring paddle, the stirring speed was set to 700 rpm and kept on, and then ammonia water and sodium hydroxide solution were added to adjust the pH value of the deionized water so that the pH value of the deionized water in the reactor was adjusted to 11.0 and the ammonia content was 1.0 g / L;
[0081] (2) The first mixed salt solution, sodium hydroxide solution and ammonia water prepared above are added to the reactor by a metering pump. The temperature of the reactor is controlled at 50°C, and a small amount of titanyl sulfate solution is continuously introduced during the reaction (the flow rate ratio with the mixed salt solution is 1:1). During the reaction, the pH value in the reactor is adjusted by the flow rate of the sodium hydroxide solution according to the growth of the particle size, so that its average value is maintained at 10.8~11.2; as the flow time increases, the particles generated by the reaction gradually grow, and the crystallinity is continuously improved. During the reaction, the slurry particle size is tested every 2 hours with a laser particle size analyzer, and the median particle size D50 of the precursor is adjusted to 3μm~5μm by adjusting the pH value in the reactor; the overflow material with qualified particle size is collected, and the overflow material flows into the aging device for aging treatment (temperature is 40°C, time is 1h~4h), and after aging, it is washed alternately with 75°C alkaline solution and pure water. The filter cake is then placed in a 120° C. forced air oven for 2 h to 5 h, and then passed through a 300-mesh sieve to obtain a powdered product, i.e., a cobalt-free single crystal manganese-rich precursor material.
[0082] (3) The obtained lithium-rich manganese precursor and lithium hydroxide are mixed in a molar ratio of Li: (Ni + Mn) = 1.3:1, and after the qualified mixture is placed in a sagger, transferred into a furnace body for sintering, the sintering temperature is 900°C, the sintering heating and cooling rates are 5°C / min, the sintering atmosphere is oxygen, and after the sintering is completed, a Ti-doped cobalt-free lithium-rich manganese-based positive electrode material is obtained.
[0083] Powder resistivity test: pressure range: 0~200MPa; 0~50MPa, interval 10MPa, 50MPa~200MPa, interval 50MPa, pressure holding 10s; measured compaction density 2.88g / cm 3 .
[0084] Comparative Example 2
[0085] This comparative example relates to a method for preparing an Al-doped lithium-rich manganese-based positive electrode material, comprising the following steps:
[0086] (1) According to the molar ratio of Ni:Mn=33:67, NiSO4·6H2O and MnSO4·H2O were weighed and dissolved in deionized water to prepare a 2 mol / L first mixed salt solution; at the same time, aluminum sulfate was weighed according to 0.5% of the total amount of Ni and Mn elements and dissolved in 600 ml of deionized water to prepare an aluminum sulfate aqueous solution, and 5 mol / L sodium hydroxide solution was prepared as a precipitant and 10 mol / L ammonia water was prepared as a complexing agent; deionized water was added to a 6 L reactor to cover the upper stirring paddle, the stirring speed was set to 700 rpm and kept on, and then ammonia water and sodium hydroxide solution were added to adjust the pH value of the deionized water so that the pH value of the deionized water in the reactor was adjusted to 11.0 and the ammonia content was 1.0 g / L;
[0087] (2) The first mixed salt solution, sodium hydroxide solution and ammonia solution prepared above are added to the reactor by a metering pump. The temperature of the reactor is controlled at 50°C, and a small amount of aluminum sulfate solution is continuously introduced during the reaction (the flow rate ratio with the mixed salt solution is 1:1). During the reaction, the pH value in the reactor is adjusted by the inlet flow rate of the sodium hydroxide solution according to the growth of the particle size, so that its average value is maintained at 10.8~11.2; as the inlet time increases, the particles generated by the reaction gradually grow, and the crystallinity is continuously improved. During the reaction, the slurry particle size is tested every 2 hours with a laser particle size analyzer. By adjusting the pH value in the reactor, the median particle size D50 of the precursor is 3μm~5μm; the overflow material with qualified particle size is collected, and the overflow material flows into the aging device for aging treatment (temperature is 40°C, time is 1h~4h). After aging, it is washed alternately with 75°C alkaline solution and pure water. The filter cake is then placed in a 120° C. forced air oven for 2 to 5 hours, and then passed through a 300-mesh sieve to obtain a powdered product, i.e., a cobalt-free single crystal manganese-rich precursor material.
[0088] (3) The obtained lithium-rich manganese precursor and lithium hydroxide are mixed in a molar ratio of Li: (Ni + Mn) = 1.3:1, and after the qualified mixture is placed in a sagger, transferred into a furnace body for sintering. The sintering temperature is 900°C, the sintering atmosphere is oxygen, and the sintering heating and cooling rates are 5°C / min. After the sintering is completed, an Al-doped cobalt-free lithium-rich manganese-based positive electrode material is obtained.
[0089] Powder resistivity test: pressure range: 0~200MPa; 0~50MPa, interval 10MPa, 50MPa~200MPa, interval 50MPa, pressure holding 10s; measured compaction density 2.72g / cm 3 .
[0090] Comparative Example 3
[0091] This comparative example relates to a method for preparing an undoped lithium-rich manganese-based positive electrode material, comprising the following steps:
[0092] (1) According to the molar ratio of Ni:Mn=33:67, NiSO4·6H2O and MnSO4·H2O were weighed and dissolved in deionized water to prepare a 2 mol / L first mixed salt solution; at the same time, 5 mol / L sodium hydroxide solution was prepared as a precipitant and 10 mol / L ammonia water was prepared as a complexing agent; deionized water was added to a 6 L reactor to cover the upper stirring paddle, the stirring speed was set to 700 rpm and kept on, and then ammonia water and sodium hydroxide solution were added to adjust the pH value of the deionized water so that the pH value of the deionized water in the reactor was adjusted to 11.0 and the ammonia content was 1.0 g / L;
[0093] (2) The first mixed salt solution, sodium hydroxide solution and ammonia water prepared above are added to the reactor by a metering pump. The temperature of the reactor is controlled at 50°C. During the reaction, the pH value in the reactor is adjusted by the flow rate of the sodium hydroxide solution according to the growth of the particle size, so that its average value is maintained at 10.8~11.2; as the flow time increases, the particles generated by the reaction gradually grow and the crystallinity is continuously improved. During the reaction, the slurry particle size is tested by a laser particle size analyzer every 2 hours. By adjusting the pH value in the reactor, the median particle size D50 of the precursor is 3μm~5μm; the overflow material with qualified particle size is collected and the overflow material flows into the aging device for aging treatment (temperature is 40°C, time is 1~4h). After aging, it is washed alternately with 75°C alkaline solution and pure water. Then the filter cake is placed in a 120°C forced air oven for 2h~5h, and then passed through a 300-mesh sieve to obtain a powdered product, i.e., a cobalt-free single crystal manganese-rich precursor material.
[0094] (3) The obtained lithium-rich manganese precursor and lithium hydroxide are mixed in a molar ratio of Li: (Ni + Mn) = 1.3:1, and after the qualified mixture is placed in a sagger, transferred into a furnace body for sintering. The sintering temperature is 900°C, the sintering atmosphere is oxygen, and the sintering heating and cooling rates are 5°C / min. After the sintering is completed, an undoped cobalt-free lithium-rich manganese-based positive electrode material is obtained.
[0095] Powder resistivity test: pressure range: 0~200MPa; 0~50MPa, interval 10MPa, 50MPa~200MPa, interval 50MPa, pressure holding 10s; measured compaction density 2.79g / cm 3 .
[0096] Comparative Example 4
[0097] (1) According to the molar ratio of Ni:Mn=33:67, NiSO4·6H2O and MnSO4·H2O were weighed and dissolved in deionized water to prepare a 2 mol / L first mixed salt solution; at the same time, titanyl sulfate and aluminum sulfate were weighed and dissolved in the first mixed salt solution according to the total amount of Ni and Mn elements of 0.2% and 0.5%, respectively, and 5 mol / L sodium hydroxide solution was prepared as a precipitant and 10 mol / L ammonia water as a complexing agent; deionized water was added to a 6 L reactor to cover the upper stirring paddle, the stirring speed was set to 700 rpm and kept on, and then ammonia water and sodium hydroxide solution were added to adjust the pH value of the deionized water so that the pH value of the deionized water in the reactor was adjusted to 11.0 and the ammonia content was 1.0 g / L;
[0098] (2) The first mixed salt solution, sodium hydroxide solution and ammonia water prepared above are added to the reactor by a metering pump. The temperature of the reactor is controlled at 50°C, and a small amount of the second mixed salt solution is continuously introduced during the reaction (the flow rate ratio with the mixed salt solution is 1:1). During the reaction, the pH value in the reactor is adjusted by the flow rate of the sodium hydroxide solution according to the growth of the particle size, so that its average value is maintained at 10.8~11.2; as the flow time increases, the particles generated by the reaction gradually grow, and the crystallinity is continuously improved. During the reaction, the slurry particle size is tested every 2 hours with a laser particle size analyzer. By adjusting the pH value in the reactor, the median particle size D50 of the precursor is 3μm~5μm; the overflow material with qualified particle size is collected, and the overflow material flows into the aging device for aging treatment (temperature is 40°C, time is 1~4h). After aging, it is washed alternately with 75°C alkaline solution and pure water. The filter cake is then placed in a 120° C. forced air oven for 2 h to 5 h, and then passed through a 300-mesh sieve to obtain a powdered product, i.e., a cobalt-free single crystal manganese-rich precursor material.
[0099] (3) The obtained cobalt-free single crystal manganese-rich precursor material and lithium hydroxide are mixed at a molar ratio of Li: (Ni + Mn) = 1.3:1, and after the qualified mixture is placed in a sagger, transferred into a furnace body for sintering, the sintering temperature is 900°C, the sintering atmosphere is oxygen, and the sintering heating and cooling rates are 5°C / min. After the sintering is completed, a cobalt-free single crystal lithium-rich manganese-based positive electrode material is obtained.
[0100] Powder resistivity test: pressure range: 0~200MPa; 0~50MPa, interval 10MPa, 50MPa~200MPa, interval 50MPa, pressure holding 10s; measured compaction density 2.48g / cm 3 .
[0101] Test example
[0102] (1) Withdrawal test: Using NMP as solvent, mix the positive electrode active material: conductive carbon black: PVDF in a ratio of 8:1:1, apply it on aluminum foil, dry it at 85°C to obtain the positive electrode sheet, and conduct the withdrawal test. The test voltage is 2.0~4.8V. The results are shown in Table 1.
[0103] (2) Compaction density test (Yuaneng Technology PRCD1100): Add the powdered positive electrode material to the equipment mold, fill the mold completely, and grind it flat. Place the mold in the equipment and start the test. During the test, apply a fixed pressure to the powder, where 0-50Mpa, maintain pressure for 10S every 10MPa, and collect data after pressure maintenance; 50-200MPa, maintain pressure for 10S every 50MPa, and collect data after pressure maintenance. Until there is no obvious change in the collected data, the limit value is the final compaction density of the material. The compaction density data is obtained, and the results are shown in Table 1.
[0104] (3) Specific surface area test: The powder sample to be tested is placed in a U-shaped sample tube, and a mixed gas containing N2 is passed through the sample. The adsorption amount of N2 by the sample to be tested is determined based on the change in gas concentration before and after adsorption. The results are shown in Table 2.
[0105] Table 1 Comparison of the charge and compaction density of lithium-rich manganese-based positive electrode materials of Examples 1 to 3 and Comparative Examples 1 to 4
[0106]
[0107] It can be seen from Table 1 that compared with comparative examples 1-4, the capacity, first effect and compaction density of the positive electrode materials prepared by the process of the present invention (Examples 1-3) are the best. This is because the precursor prepared under the process conditions has a larger specific surface area, is in sufficient contact with the lithium salt during the sintering process, and reacts more completely, forming a lithium-rich manganese-based single crystal positive electrode material with excellent performance.
[0108] Table 2 Comparison of specific surface areas of lithium-rich manganese-based precursors of Examples 1 to 3 and Comparative Examples 1 to 4
[0109]
[0110] It can be seen from Table 2 that, compared with Comparative Examples 1-4, the precursors treated by the process of the present invention (Examples 1-3) have a larger specific surface area and a larger contact area after mixing with the lithium salt, which is beneficial for subsequent sintering and lithium insertion.
[0111] in, Figure 1 This is a SEM image of the lithium-rich manganese-based positive electrode material prepared in Example 1 of the present invention, wherein Figure 1 It was taken under Regulus8100 5.0kV 8.8mmx10.0k SE (UL) conditions; Figure 2 This is a diagram of a Ti-doped lithium-rich manganese-based positive electrode material prepared in Comparative Example 1 of the present invention, wherein Figure 2 It was taken under Regulus8100 5.0kV 5.5mmx10.0k SE (UL) conditions; Figure 3 This is a diagram of the Al-doped lithium-rich manganese-based positive electrode material prepared in Comparative Example 2 of the present invention, wherein Figure 3 It was taken under Regulus81005.0kV 8.7mmx10.0k SE (UL) conditions; Figure 4 This is a diagram of an undoped lithium-rich manganese-based positive electrode material prepared in Comparative Example 3 of the present invention, wherein Figure 4 The images were taken under Regulus8100 5.0kV 8.5mmx10.0k SE (UL) conditions. Figures 1 to 4 It can be seen that the precursor prepared by the process of the present invention can be sintered to form a uniformly dispersed lithium-rich manganese-based single crystal positive electrode material, while a uniformly dispersed lithium-rich manganese-based single crystal positive electrode cannot be prepared under other process conditions. This shows that the precursor preparation process has a direct impact on the lithium-rich manganese-based single crystal positive electrode, thereby illustrating the innovativeness of the process of the present invention.
[0112] In summary, the present invention optimizes the precursor preparation process and the precursor in-situ doping process to effectively improve the contact area between the precursor and the lithium salt during the sintering process, thereby preparing a cobalt-free single crystal lithium-manganese-rich positive electrode material without changing the positive electrode material preparation process, and the prepared cobalt-free single crystal lithium-manganese-rich positive electrode material has significant advantages in withholding capacity, initial particle efficiency and compaction density.
[0113] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0114] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing a lithium-rich manganese-based precursor, characterized in that: The method comprises the following steps: forming a core of a lithium-rich manganese-based precursor by a precipitation reaction of a first mixed salt solution, and then adding a second mixed salt solution to continue the precipitation reaction to form a lithium-rich manganese-based precursor; the first mixed salt comprises a nickel salt and a manganese salt; the second mixed salt comprises an aluminum salt and a titanium salt; The titanium salt includes at least one of TiOSO4, Ti2O3(SO4), and Ti4O5(SO4)3; The molar ratio of the nickel element in the nickel salt to the manganese element in the manganese salt is 25:75-40:60; the aluminum element in the aluminum salt accounts for 0.4%-0.6% of the total amount of the nickel element in the nickel salt and the manganese element in the manganese salt; the titanium element in the titanium salt accounts for 0.1%-0.3% of the total amount of the nickel element in the nickel salt and the manganese element in the manganese salt; The lithium-rich manganese-based precursor does not contain Co element; The parameters of the precipitation reaction are as follows: the reaction temperature is 45° C. to 55° C., the stirring speed is 400 rpm to 900 rpm, and the pH is 10.8 to 11.
2.
2. The method for preparing a lithium-rich manganese-based precursor according to claim 1, characterized in that: The particle size D50 of the core of the lithium-rich manganese-based precursor is 0.8 μm to 1.2 μm; the particle size D50 of the lithium-rich manganese-based precursor is 3 μm to 5 μm; And / or, the nickel salt includes at least one of nickel sulfate and nickel nitrate; And / or, the manganese salt includes at least one of manganese sulfate and manganese nitrate; And / or, the aluminum salt includes at least one of aluminum sulfate and aluminum nitrate.
3. The method for preparing a lithium-rich manganese-based precursor according to claim 1, characterized in that: The method comprises the following specific steps: adding a precipitant and a complexing agent to a first mixed salt solution to carry out a precipitation reaction to form a core of a lithium-rich manganese-based precursor, then adding a second mixed salt solution, a precipitant and a complexing agent to continue to carry out a precipitation reaction to form a lithium-rich manganese-based precursor, and then aging, washing and drying in sequence to obtain a lithium-rich manganese-based precursor; The precipitant includes at least one of sodium hydroxide and potassium hydroxide; the complexing agent includes at least one of ammonia water and ammonium sulfate; The concentration of the complexing agent is 5 mol / L to 15 mol / L.
4. A lithium-rich manganese-based precursor, characterized in that: The lithium-rich manganese-based precursor is prepared by the preparation method according to any one of claims 1 to 3.
5. A lithium-rich manganese-based positive electrode material, characterized in that: The lithium-rich manganese-based positive electrode material is prepared from the lithium-rich manganese-based precursor according to claim 4.
6. A method for preparing a lithium-rich manganese-based positive electrode material according to claim 5, characterized in that: The method comprises the following steps: mixing the lithium-rich manganese-based precursor according to claim 4 with a lithium salt and sintering the mixture to obtain a lithium-rich manganese-based positive electrode material.
7. The preparation method according to claim 6, characterized in that: The ratio of the total amount of nickel and manganese in the lithium-rich manganese-based precursor to the amount of lithium in the lithium salt is 1:1.2-1.45; The lithium salt includes at least one of lithium carbonate and lithium chloride; The sintering parameters are as follows: sintering temperature is 850° C. to 1000° C., sintering time is 8 h to 18 h, sintering atmosphere is oxygen, and sintering heating and cooling rates are 1° C. / min to 10° C. / min.
8. A lithium ion battery, characterized in that: The lithium-ion battery comprises the lithium-rich manganese-based positive electrode material according to claim 5.