A low water peak optical fiber preform helium-free sintering device and use method thereof
By adopting the separation structure of molybdenum heating rod and silicon carbide furnace tube in the optical fiber preform sintering equipment, combining nitrogen protection and vacuum pump group control, helium-free sintering is achieved, solving the problems of high helium usage and poor equipment stability, and improving Dehydroxylation efficiency and product quality.
Patent Information
- Application Number
- CN202411081766.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-08
AI Technical Summary
During the use of existing fiber preform sintering equipment, there are problems such as high helium usage, poor equipment stability, and low dehydroxylation efficiency, and helium-free sintering cannot be achieved, resulting in poor production costs and product quality.
A low-water peak fiber prefabricated rod prefabricated rod is designed, and the main furnace body and interlayer cavity structure is separated by molybdenum heating rod and silicon carbide furnace tube. The gas is protected by a tungsten insulation screen and nitrogen, and a vacuum pump group and a pneumatic valve are used. The control system realizes helium-free sintering, ensuring independent pressure management of the interlayer chamber and load chamber, and achieving efficient degassing and vitrification processes.
The device realizes helium-free sintering, improves the stability and dehydroxylation efficiency of the equipment, significantly reduces the production cycle and cost, and ensures high-quality production of low-water peak fiber preform rods.
Smart Images

Figure CN118598501B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of optical fiber communication, and in particular relates to a low-water-peak optical fiber preform helium-free sintering device and a use method thereof. Background Art
[0002] In the field of optical fiber preform manufacturing and sintering, sintering equipment is mainly divided into normal pressure and negative pressure sintering equipment. The furnace structure is basically a sintering product container in the middle, heating components are installed around the sintering product container, and heat insulation devices are installed around the heating components and equipped with corresponding contact or non-contact temperature measurement components. The heating method is mainly electric heating, and the heating components usually use graphite heating, induction heating, and plasma heating. Among them, graphite heating is the most used. Induction heating and plasma heating are relatively less used due to cost issues and current technical issues. However, the use of graphite heating has the following defects:
[0003] Most of the insulation materials for sintering equipment are made of graphite. Graphite has excellent thermal insulation properties. However, as the use time increases, the graphite will gradually pulverize due to oxidation, resulting in an increase in graphite dust in the furnace, which not only affects product quality, but also causes serious equipment short circuits and damage, seriously affecting product quality and equipment stability.
[0004] In order to alleviate the above problems, a Chinese patent, with publication number CN211497392U, is entitled "A low-helium anti-oxidation device for a preform sintering furnace". It discloses that an inert gas inlet pipe and a helium inlet pipe are respectively arranged at the bottom and top of the left side of the sintering furnace wall, the helium inlet pipe is connected to the left side of the furnace core tube, a connecting pipe is provided with a plurality of branches with control valves, and the connecting pipes are respectively connected to the bottom of the preparation room, the top and bottom of the right side of the furnace core tube, and the right side of the sintering furnace wall, the connecting pipe is connected to a vacuum pump and through vacuum suction, a flow field is formed in which gas flows from the bottom to the top in the area between the inner wall of the sintering furnace wall and the outer side of the graphite insulation part, the lower end of the preparation room is connected to the upper end of the furnace core tube and an isolation valve is arranged at the connection, which has the advantages of low helium usage and high helium utilization, and the flow field can effectively isolate the air to prevent oxidation of graphite parts and increase the service life of the equipment. However, the above patent only solves the problem of graphite part oxidation, fails to achieve helium-free sintering, and does not meet the requirements for producing low water peak optical fiber preforms.
[0005] In the field of optical fiber preform sintering, due to the shortage of helium energy, the unit price of helium continues to rise, resulting in a substantial increase in the manufacturing cost of optical fiber preforms. Therefore, helium-free sintering is a difficult problem that must be overcome in the field of optical fiber preform sintering. The Chinese invention patent, publication number CN114014532A, is entitled "A low-helium sintering device for optical fiber preform powder sintering process". It discloses reducing the amount of helium used in atmospheric pressure sintering by improving the gas sealing of the device, but the patent cannot fundamentally solve the problem of using helium.
[0006] Chinese invention patent, publication number CN101781087A, patent name is a kind of loose body optical fiber preform integrated sintering degassing equipment and method, discloses the introduction of chlorine in the dehydroxylation stage, and the introduction of helium and deuterium in the vitrification stage, but the patent cannot achieve helium-free sintering, cannot control the dehydroxylation pressure level, and has low dehydroxylation efficiency. At the same time, the above patent discloses that dehydroxylation should be performed preferentially at a temperature of 1100℃~1150℃, but due to the high temperature limit of its sintering equipment itself, it is necessary to feed the rod while dehydroxylation through the rod feeding mechanism, because the optical fiber preform has a significant difference in residence time in the chlorine atmosphere, resulting in a large difference in the chlorine content of the cladding, resulting in a higher chlorine content at the end of the rod than at the top. The above patent also discloses that it is necessary to heat up during the vitrification process, control the evacuation pressure at 400mbar~500mbar, and gradually control the rod feeding mechanism to gradually complete the vitrification of the entire optical rod, which has high requirements for the furnace tube strength and potential safety hazards. The above patent also discloses the use of carbon furnace core tubes, which have oxidation problems as the service life is prolonged. The loose body will have trace amounts of oxygen during the dehydroxylation and degassing process, causing the cleanliness inside the tube to gradually deteriorate as the service life is prolonged, ultimately leading to poor product quality.
[0007] Therefore, how to save helium while taking into account the efficiency of blanket dehydroxylation is a key issue that the industry urgently needs to solve. Summary of the invention
[0008] In order to solve the technical problems existing in the prior art, the object of the present invention is to provide a low water peak optical fiber preform helium-free sintering device and a use method thereof.
[0009] In order to achieve the above purpose and the above technical effect, the technical solution adopted by the present invention is:
[0010] A low water peak optical fiber preform helium-free sintering device, comprising:
[0011] The main furnace body comprises a loading cavity and an interlayer cavity outside thereof, wherein an optical fiber preform for production is arranged in the loading cavity, and a heating device for heating the optical fiber preform is arranged in the interlayer cavity, and the pressure of the loading cavity is greater than the pressure of the interlayer cavity;
[0012] The exhaust system in the furnace includes a loading chamber exhaust system communicating with the loading chamber and an interlayer chamber exhaust system communicating with the interlayer chamber. The exhaust function of the loading chamber is realized through the loading chamber exhaust system, and the exhaust function of the interlayer chamber is realized through the interlayer chamber exhaust system.
[0013] Furthermore, the loading chamber and the interlayer chamber are separated by a silicon carbide furnace tube, the heating device is a molybdenum heating rod, and a furnace body tungsten heat insulation screen is arranged in the interlayer chamber and around the molybdenum heating rod.
[0014] Furthermore, the loading chamber exhaust system includes a loading chamber air duct, which includes a main line and a branch line, and the main line and the branch line are respectively connected to the exhaust duct, and the main line is provided with a loading chamber pressure control valve and a loading chamber exhaust pneumatic valve, and the branch line is provided with a loading chamber vacuum pipeline pneumatic valve and a loading chamber vacuum pump group.
[0015] Furthermore, the interlayer chamber exhaust system includes an interlayer chamber air duct, which is connected to an exhaust duct. The interlayer chamber air duct is provided with an interlayer nitrogen gas intake pneumatic valve, an interlayer chamber pressure control valve, an interlayer chamber vacuum pipeline pneumatic valve and an interlayer chamber exhaust pneumatic valve. The interlayer nitrogen gas intake pneumatic valve is arranged between the interlayer chamber air duct and a gas mass flow controller, the interlayer chamber vacuum pipeline pneumatic valve is arranged between the interlayer chamber air duct and an interlayer chamber vacuum pump group, and the interlayer chamber vacuum pump group is also connected to the exhaust duct.
[0016] Furthermore, the exhaust duct is connected to the main air duct, and the main air duct is used to realize the function of transporting the waste gas in the interlayer cavity and the loading cavity.
[0017] Furthermore, the optical fiber preform is connected to one end of a sintering guide rod through a connecting sleeve, and the other end of the sintering guide rod is arranged on an equipment tower. The interior of the sintering guide rod is hollow and communicates with a loading chamber, so that the optical fiber preform can be fed and lifted from top to bottom or from bottom to top through the sintering guide rod.
[0018] Furthermore, the loading chamber is connected to the gas mixing device through the sintering guide rod, and an upper loading air intake pneumatic valve is provided between the sintering guide rod and the gas mixing device, and the gas ratio of the loading chamber intake is regulated by the gas mixing device.
[0019] Furthermore, a sintering upper sealing device is provided on the top of the main furnace body, which is used to achieve sealing with the sintering guide rod and sealing with the furnace mouth of the main furnace body.
[0020] Furthermore, the main furnace body is provided with a loading chamber pressure gauge, an interlayer chamber pressure gauge and an infrared thermocouple. The loading chamber pressure gauge is communicated with the loading chamber, and real-time monitoring of the loading chamber pressure is achieved through the loading chamber pressure gauge. The interlayer chamber pressure gauge is communicated with the interlayer chamber, and real-time monitoring of the interlayer chamber pressure is achieved through the interlayer chamber pressure gauge. Real-time monitoring of the temperature inside the main furnace body is achieved through the infrared thermocouple.
[0021] The present invention also discloses a method for using a low water peak optical fiber preform helium-free sintering device, comprising the following steps:
[0022] First, confirm that the rod hanging point is at the zero point, that is, the sintering guide rod and the connecting sleeve are at the specified position; then, hang the optical fiber preform on the connecting sleeve; start to enter the production state, control the optical fiber preform to enter the production position, during the rod feeding process, the molybdenum heating rod is maintained at a temperature of 500℃~1100℃, and the interlayer cavity is always in an inert gas protection atmosphere. After the optical fiber preform is fed to the production position, the effective section of the optical fiber preform enters the effective position of the temperature zone and is located at the center of the temperature zone. At this time, the sintering upper sealing device forms a seal with the main furnace body furnace mouth. First, the sintering guide rod is controlled by the motor to drive the optical fiber preform to rotate, with a speed of 0.5rpm~20rpm, and then the interlayer chamber is opened to exhaust air synchronously. Open the pneumatic valve and the exhaust pneumatic valve of the loading chamber, and control the air pressure at -200Pa~-600Pa. Open the interlayer chamber pressure control valve and the loading chamber pressure control valve simultaneously. Set the loading chamber pressure at 50Pa~2000Pa. Monitor it through the loading chamber pressure gauge and monitor the interlayer chamber pressure through the interlayer chamber pressure gauge to ensure that the loading chamber pressure is always greater than the interlayer chamber pressure. After maintaining it for 30min~500min, heat it to the target temperature at the set slope of 0℃ / min~8℃ / min. Use an infrared thermocouple to monitor the temperature in the main furnace in real time. After the heating is completed, continue to maintain it for 30min~600min. After the above steps are completed, enter the degassing and vitrification stage:
[0023] First, close the interlayer chamber exhaust pneumatic valve, loading chamber exhaust pneumatic valve, and interlayer nitrogen inlet pneumatic valve, and simultaneously open the interlayer chamber vacuum pipeline pneumatic valve and loading chamber vacuum pipeline pneumatic valve, and simultaneously open the interlayer chamber vacuum pump group and loading chamber vacuum pump group, and synchronously decompress and evacuate the loading chamber and the interlayer chamber. The synchronous furnace temperature is raised to 1520℃~1560℃ at a set slope of 2℃ / min~5℃ / min to vitrify the optical fiber preform. In terms of mass percentage, the process gas is nitrogen 90%~98%, chlorine 2%~10%, and the vacuum degree of the loading chamber should be slightly lower than that of the interlayer chamber, and the control range is 0. pa~3000pa, PID control is performed through the interlayer chamber pressure control valve and the loading chamber pressure control valve. After vitrification is completed, the interlayer chamber vacuum pipeline pneumatic valve and the loading chamber vacuum pipeline pneumatic valve are closed synchronously, and the interlayer chamber vacuum pump group, the loading chamber vacuum pump group, the interlayer chamber pressure control valve, and the loading chamber pressure control valve are closed with delay. The interlayer nitrogen gas inlet pneumatic valve is opened, and the interlayer chamber air intake volume is variable, and the loading air intake volume is 1L / min~5L / min. Then, the gas mass flow controller is regulated by PLC to ensure that the absolute value of the pressure difference between the loading chamber pressure gauge and the interlayer chamber pressure gauge is within 0pa~3000pa. After the pressurization is completed, the temperature is cooled synchronously to the standby temperature of 800℃, and the product is lifted to the rod hanging and taking point through the sintering guide rod and the connecting sleeve, and the production department is notified to take the rod to complete this production.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] The invention discloses a low-water-peak optical fiber preform helium-free sintering device and a use method thereof. The overall structure is simple and the use is convenient. The device can efficiently complete the process of dehydroxylation, degassing and vitrification, and pressurized rod taking, fundamentally solving the problem of the gradual deterioration of the cleanliness of the chamber of the optical fiber preform sintering equipment as the use time increases, and at the same time solving the problem of low dehydroxylation efficiency in the field of helium-free sintering technology, and can obtain a low OH- cladding in a relatively shorter time, greatly reducing the production cycle and cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a structural schematic diagram of the present invention;
[0027] Figure 2 It is a flow chart of the present invention. DETAILED DESCRIPTION
[0028] The present invention is described in detail below so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.
[0029] A brief summary of one or more aspects is given below to provide a basic understanding of these aspects. This summary is not an exhaustive overview of all conceived aspects, and is neither intended to identify the key or critical elements of all aspects nor to define the scope of any or all aspects. Its only purpose is to give some concepts of one or more aspects in a simplified form as a prelude to a more detailed description that will be given later.
[0030] like Figure 1 As shown, the present invention discloses a helium-free sintering device for a low water peak optical fiber preform, comprising:
[0031] The sintering guide rod 1 is hollow inside and is used to realize the feeding and lifting action of the optical fiber preform rod 6 from top to bottom or from bottom to top and drive the optical fiber preform rod 6 to rotate at a certain speed. The sintering guide rod 1 is communicated with the loading cavity of the main furnace body;
[0032] A loading chamber pressure gauge 2, which is in communication with the loading chamber and is used to monitor the pressure of the loading chamber in real time;
[0033] The sintering upper sealing device 3 is used to achieve sealing with the sintering guide rod 1 and sealing with the main furnace body furnace mouth;
[0034] The interlayer chamber pressure gauge 4 is communicated with the interlayer chamber of the main furnace body and is used to realize real-time monitoring of the interlayer chamber pressure;
[0035] A connecting sleeve 5, used to connect the sintering guide rod 1 with the optical fiber preform 6;
[0036] Optical fiber preform 6;
[0037] The molybdenum heating rod 7 is arranged in the interlayer cavity and is used to convert electrical energy into thermal energy to heat the optical fiber preform 6 to a desired temperature;
[0038] The furnace body tungsten heat shield 8 is arranged in the interlayer cavity and outside the molybdenum heating rod 7;
[0039] Silicon carbide furnace tube 9, used to realize the division of the loading chamber and the interlayer chamber of the main furnace body;
[0040] Infrared thermocouple 10, used to achieve real-time monitoring of the temperature of the outer wall of the main furnace body, that is, to achieve real-time monitoring of the temperature of the main furnace body;
[0041] The equipment tower 11 is used to realize the support function of equipment installation and product transportation. When in use, the sintering guide rod 1 is arranged on the equipment tower 11, so as to facilitate the hanging of the optical fiber preform 6 in the loading chamber. The sintering guide rod 1 can realize the feeding and lifting action of the optical fiber preform 6 from top to bottom or from bottom to top;
[0042] The upper loading air intake pneumatic valve 12 is used to realize the opening and closing functions of the loading chamber air intake;
[0043] A gas mixing device 13 is connected to the loading chamber through the sintering guide rod 1. A loading upper air intake pneumatic valve 12 is provided between the gas mixing device 13 and the sintering guide rod 1. The gas mixing device 13 realizes the gas ratio control function of the loading chamber air intake.
[0044] The main air duct 14 is used to realize the function of transporting the waste gas from the interlayer cavity and the loading cavity;
[0045] A gas mass flow controller 15 is used to achieve a precise control function of the gas intake into the interlayer cavity;
[0046] The interlayer nitrogen gas inlet pneumatic valve 16 is used to realize the opening and closing functions of the interlayer cavity gas inlet;
[0047] Exhaust pipe 17, used to realize exhaust transportation function;
[0048] The interlayer chamber air duct 18 is used to realize the interlayer chamber exhaust function;
[0049] The sandwich chamber pressure control valve 19 is used to realize the sandwich chamber pressure control function and the loading exhaust opening and closing function;
[0050] The interlayer chamber exhaust pneumatic valve 20 is used to realize the opening and closing functions of the main exhaust of the interlayer chamber;
[0051] The pneumatic valve 21 of the vacuum pipeline of the sandwich chamber is used to realize the on-off function of exhaust;
[0052] The interlayer chamber vacuum pump group 22 is used to realize the interlayer chamber exhaust function;
[0053] The loading chamber air duct 23 includes a main circuit and a branch circuit. A loading chamber pressure control valve 24 and a loading chamber exhaust pneumatic valve 25 are provided on the main circuit. A loading chamber vacuum pipeline pneumatic valve 26 and a loading chamber vacuum pump group 27 are provided on the branch circuit. The loading chamber pressure control valve 24 is used to realize the loading chamber pressure control function and the loading exhaust opening and closing function. The loading chamber exhaust pneumatic valve 25 is used to realize the loading chamber exhaust opening and closing function. The loading chamber vacuum pipeline pneumatic valve 26 is used to realize the loading chamber exhaust switch function. The loading chamber vacuum pump group 27 is used to realize the loading chamber exhaust function.
[0054] In the present invention, the exhaust duct 17, the interlayer chamber air duct 18 and the loading chamber air duct 23 constitute an exhaust pipe system, one end of the exhaust duct 17 is connected to the main air duct 14, and the other end of the exhaust duct 17 is respectively connected to the interlayer chamber air duct 18 and the loading chamber air duct 23, the interlayer chamber air duct 18 is also connected to the interlayer cavity, and the loading chamber air duct 23 is also connected to the loading cavity. The interlayer chamber air duct 18 is provided with an interlayer nitrogen gas intake pneumatic valve 16, an interlayer chamber pressure control valve 19, an interlayer chamber vacuum pipeline pneumatic valve 21 and an interlayer chamber exhaust pneumatic valve 20, the interlayer nitrogen gas intake pneumatic valve 16 is arranged between the interlayer chamber air duct 18 and the gas mass flow controller 15, the interlayer chamber vacuum pipeline pneumatic valve 21 is arranged between the interlayer chamber air duct 18 and the interlayer chamber vacuum pump group 22, and the interlayer chamber vacuum pump group 22 is also connected to the exhaust duct 17.
[0055] like Figure 2 As shown, the present invention also discloses a method for using a low water peak optical fiber preform helium-free sintering device, comprising the following steps:
[0056] First, confirm that the rod hanging point is at the zero point, that is, the sintering guide rod 1 and the connecting sleeve 5 are at the specified position. Then, hang the optical fiber preform 6 on the connecting sleeve 5. Enter the production state, control the optical fiber preform 6 to advance to the production position, during the rod advancement process, the molybdenum heating rod 7 is maintained at a temperature of 500°C~1100°C, and the interlayer cavity is always kept in an inert gas protective atmosphere. After the optical fiber preform 6 is advanced to the production position, the effective section of the optical fiber preform 6 enters the effective position of the temperature zone and is located in the center of the temperature zone. At this time, the sintering upper sealing device 3 forms a seal with the furnace mouth. First, the sintering guide rod 1 is controlled by the motor to drive the optical fiber preform 6 to rotate at a speed of 0.5rpm~20rpm, and then it is synchronously hit. Open the interlayer chamber exhaust pneumatic valve 20 and the loading chamber exhaust pneumatic valve 25, control the air pressure at -200Pa~-600Pa, and simultaneously open the interlayer chamber pressure control valve 19 and the loading chamber pressure control valve 24, set the loading chamber pressure at 50Pa~2000Pa, and monitor it through the loading chamber pressure gauge 2. The interlayer chamber pressure setting value is 200Pa~2000Pa, and the interlayer chamber pressure is monitored by the interlayer chamber pressure gauge 4. The loading chamber and the interlayer chamber always keep the loading chamber pressure greater than the interlayer chamber pressure, and the loading chamber and the interlayer chamber are independent of each other. Among them, the source of maintaining the pressure difference in the loading chamber is the use of process gas in the loading chamber. By opening the loading lower air inlet pneumatic valve 12 and setting the ratio of the gas mixing device 13, the process gas contains 75%~95% nitrogen and 5%~25% chlorine. The main source of interlayer cavity pressure control is nitrogen (99.999%). The gas flow rate is controlled by opening the interlayer nitrogen inlet pneumatic valve 16 and the gas mass flow controller 15 to maintain the interlayer cavity pressure. After maintaining for 30min~500min, the temperature is raised to the target temperature (1100℃~1300℃) according to the set slope of 0℃ / min~8℃ / min. The infrared thermocouple 10 is used to monitor the loading cavity temperature in real time. After the temperature is raised, it is maintained for 30min~600min. After the above steps are completed, the degassing and vitrification stage is entered:
[0057] First, close the interlayer chamber exhaust pneumatic valve 20, the loading chamber exhaust pneumatic valve 25, and the interlayer nitrogen inlet pneumatic valve 16, and simultaneously open the interlayer chamber vacuum pipeline pneumatic valve 21 and the loading chamber vacuum pipeline pneumatic valve 26, and simultaneously open the interlayer chamber vacuum pump group 22 and the loading chamber vacuum pump group 27, and synchronously decompress and evacuate the loading chamber and the interlayer chamber. The synchronous furnace temperature is raised to 1520℃~1560℃ at a set slope of 2℃ / min~5℃ / min to vitrify the optical fiber preform 6. The process gases are nitrogen (90%~98%) and chlorine (2%~10%). The vacuum degree of the loading chamber should be slightly lower than that of the interlayer chamber, and the control range is 0 pa~3000pa, PID control is performed through the interlayer chamber pressure control valve 19 and the loading chamber pressure control valve 24, and after vitrification is completed, the interlayer chamber vacuum pipeline pneumatic valve 21 and the loading chamber vacuum pipeline pneumatic valve 26 are closed synchronously, and the interlayer chamber vacuum pump group 22, the loading chamber vacuum pump group 27, the interlayer chamber pressure control valve 19, and the loading chamber pressure control valve 24 are closed with delay, and the interlayer nitrogen gas inlet pneumatic valve 16 is opened. The interlayer chamber gas intake volume is a variable, and the loading gas intake volume is 1L / min~5L / min. Then, the gas mass flow controller 15 is regulated by PLC to ensure that the absolute value of the pressure difference between the loading chamber pressure gauge 2 and the interlayer chamber pressure gauge 4 is within 0pa~3000pa. After the pressurization is completed, the temperature is cooled synchronously to the standby temperature of 800℃, and the product is lifted to the rod hanging and taking point through the sintering guide rod 1 and the connecting sleeve 5, and the production department is notified to take the rod to complete this production.
[0058] Example 1
[0059] First, confirm that the rod hanging point is at the zero point, that is, the sintering guide rod 1 and the connecting sleeve 5 are at the specified position. Then, the optical fiber preform rod 6 is hung on the connecting sleeve 5. Entering the production state, the servo motor is controlled by PLC to drive the optical fiber preform 6 to advance to the production position. During the rod advancement process, the molybdenum heating rod 7 is maintained at a temperature of 900°C, and the interlayer cavity is kept in an inert gas protective atmosphere. After the optical fiber preform 6 is advanced to the production position, the effective section of the optical fiber preform 6 enters the effective position of the temperature zone and is located at the center of the temperature zone. At this time, the sintering upper sealing device 3 forms a seal with the furnace mouth. First, the sintering guide rod 1 is controlled by the motor to drive the optical fiber preform 6 to rotate at a speed of 5 rpm. The interlayer chamber exhaust pneumatic valve 20 and the loading chamber exhaust pneumatic valve 25 are opened synchronously, and the wind pressure is controlled at -350 Pa. The interlayer chamber pressure control valve 19 and the loading chamber pressure control valve 24 are opened synchronously, and the loading chamber pressure is set at 280 Pa, which is monitored by the loading chamber pressure gauge 2. The interlayer chamber pressure is set at 260 Pa, and the interlayer chamber pressure is monitored by the interlayer chamber pressure gauge 4, so that the loading chamber pressure is always kept greater than the interlayer chamber pressure. Among them, the source of maintaining the pressure difference in the loading chamber is the process gas used in the loading chamber. By opening the lower air inlet pneumatic valve 12 of the loading chamber and setting the ratio of the gas mixing device 13, the process gas contains 85% nitrogen and 15% chlorine. The main source of interlayer chamber pressure control is nitrogen (99.999%). The gas intake is controlled by opening the interlayer nitrogen air inlet pneumatic valve 16 and the gas mass flow controller 15 to maintain the pressure of the interlayer chamber. After maintaining for 150 minutes, the temperature is raised to the target temperature of 1250°C at a set slope of 4°C / min, and monitored by an infrared thermocouple 10. After the temperature is raised, it is maintained for 200 minutes. After the above-mentioned dehydroxylation step is completed, the degassing and vitrification stages are continued:
[0060] First, close the interlayer chamber exhaust pneumatic valve 20, the loading chamber exhaust pneumatic valve 25, and the interlayer nitrogen inlet pneumatic valve 16, and simultaneously open the interlayer chamber vacuum pipeline pneumatic valve 21 and the loading chamber vacuum pipeline pneumatic valve 26, and simultaneously open the interlayer chamber vacuum pump group 22 and the loading chamber vacuum pump group 27, and synchronously decompress and evacuate the loading chamber and the interlayer chamber, and synchronously increase the furnace temperature to 1520°C at a set slope of 2°C / min to perform vitrification of the optical fiber preform 6, wherein the process gas is nitrogen 98% and chlorine 2%, and the vacuum degree of the loading chamber should be slightly lower than that of the interlayer chamber, and the control range is 1600Pa. PID control is performed through the interlayer chamber pressure control valve 19 and the loading chamber pressure control valve 24. After the vitrification is completed, the interlayer chamber vacuum pipeline pneumatic valve 21 is synchronously closed. Valve 21 and loading chamber vacuum pipeline pneumatic valve 26, delay closing interlayer chamber vacuum pump group 22, loading chamber vacuum pump group 27, interlayer chamber pressure control valve 19, loading chamber pressure control valve 24, open interlayer nitrogen gas inlet pneumatic valve 16, the interlayer chamber air intake volume is variable, the loading chamber air intake volume is a fixed value of 1.5L / min, and then the gas mass flow controller 15 is regulated by PLC to ensure that the absolute value of the pressure difference between the loading chamber pressure gauge 2 and the interlayer chamber pressure gauge 4 is within 1600Pa. After the pressurization is completed, the temperature is cooled synchronously to the standby temperature of 800℃, and the product is lifted to the rod hanging point through the sintering guide rod 1 and the connecting sleeve 5, and the production department is notified to take the rod to complete this production. The hydroxyl content of the test sample is ≤6.50μg / g.
[0061] Example 2
[0062] First, confirm that the rod hanging point is at the zero point, that is, the sintering guide rod 1 and the connecting sleeve 5 are at the specified position. Then, the optical fiber preform rod 6 is hung on the connecting sleeve 5. Entering the production state, the servo motor is controlled by PLC to drive the optical fiber preform 6 to advance to the production position. During the rod advancement process, the molybdenum heating rod 7 is maintained at a temperature of 900°C, and the interlayer cavity is kept in an inert gas protective atmosphere. After the optical fiber preform 6 is advanced to the production position, the effective section of the optical fiber preform 6 enters the effective position of the temperature zone and is located at the center of the temperature zone. At this time, the sintering upper sealing device 3 forms a seal with the furnace mouth. First, the sintering guide rod 1 is controlled by the motor to drive the optical fiber preform 6 to rotate at a speed of 5 rpm. The interlayer chamber exhaust pneumatic valve 20 and the loading chamber exhaust pneumatic valve 25 are opened synchronously, and the wind pressure is controlled at -350 Pa. The interlayer chamber pressure control valve 19 and the loading chamber pressure control valve 24 are opened synchronously, and the loading chamber pressure is set at 280 Pa, which is monitored by the loading chamber pressure gauge 2. The interlayer chamber pressure is set at 260 Pa, and the interlayer chamber pressure is monitored by the interlayer chamber pressure gauge 4, so that the loading chamber pressure is always kept greater than the interlayer chamber pressure. Among them, the source of maintaining the pressure difference in the loading chamber is the process gas used in the loading chamber. By opening the lower air inlet pneumatic valve 12 of the loading chamber and setting the ratio of the gas mixing device 13, the process gas contains 85% nitrogen and 15% chlorine. The main source of interlayer chamber pressure control is nitrogen (99.999%). The gas intake is controlled by opening the interlayer nitrogen air inlet pneumatic valve 16 and the gas mass flow controller 15 to maintain the pressure of the interlayer chamber. After maintaining for 200 minutes, the temperature is raised to the target temperature of 1250°C at a set slope of 4°C / min, and monitored by an infrared thermocouple 10. After the temperature is raised, it is maintained for 300 minutes. After the above-mentioned dehydroxylation step is completed, the degassing and vitrification stages are continued:
[0063] First, close the interlayer chamber exhaust pneumatic valve 20, the loading chamber exhaust pneumatic valve 25, and the interlayer nitrogen inlet pneumatic valve 16, and simultaneously open the interlayer chamber vacuum pipeline pneumatic valve 21 and the loading chamber vacuum pipeline pneumatic valve 26, and simultaneously open the interlayer chamber vacuum pump group 22 and the loading chamber vacuum pump group 27, and synchronously decompress and evacuate the loading chamber and the interlayer chamber, and synchronously increase the furnace temperature to 1520°C at a set slope of 2°C / min to perform vitrification of the optical fiber preform 6, wherein the process gas is nitrogen 98% and chlorine 2%, and the vacuum degree of the loading chamber should be slightly lower than that of the interlayer chamber, and the control range is 1600Pa. PID control is performed through the interlayer chamber pressure control valve 19 and the loading chamber pressure control valve 24. After the vitrification is completed, the interlayer chamber vacuum pipeline pneumatic valve 21 is synchronously closed. Valve 21 and pneumatic valve 26 of vacuum pipeline of loading chamber, delay closing of vacuum pump group 22 of interlayer chamber, vacuum pump group 27 of loading chamber, pressure control valve 19 of interlayer chamber, pressure control valve 24 of loading chamber, open pneumatic valve 16 of nitrogen inlet of interlayer, air intake of interlayer chamber is variable, air intake of loading chamber is fixed value 1.5L / min, then regulate the amount of gas mass flow controller 15 through PLC, to ensure that the pressure difference absolute value of pressure gauge 2 of loading chamber and pressure gauge 4 of interlayer chamber is within 1600pa, wait for pressurization to be completed, start cooling synchronously, cool to standby temperature 800℃, lift product rod to the rod hanging point through sintering guide rod 1 and connecting sleeve 5, notify production department to take rod, complete this production, test sample hydroxyl content ≤0.50μg / g. Due to the extended chlorination time of this embodiment, the hydroxyl content of this embodiment is lower than that of embodiment 1, indicating that chlorination time will affect the hydroxyl content of sample.
[0064] Parts or structures not specifically described in the present invention may adopt existing technologies or existing products and will not be described in detail here.
[0065] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for using a low water peak optical fiber preform helium-free sintering device, characterized in that: The low water peak optical fiber preform helium-free sintering device comprises: The main furnace body comprises a loading cavity and an interlayer cavity outside thereof, wherein an optical fiber preform for production is placed in the loading cavity, and a heating device for heating the optical fiber preform is arranged in the interlayer cavity, and the pressure of the loading cavity is greater than the pressure of the interlayer cavity; The exhaust system in the furnace includes a loading chamber exhaust system communicating with the loading chamber and an interlayer chamber exhaust system communicating with the interlayer chamber. The exhaust function of the loading chamber is realized by the loading chamber exhaust system, and the exhaust function of the interlayer chamber is realized by the interlayer chamber exhaust system. The method of use comprises the following steps: First, confirm that the rod hanging point is at the zero point, that is, the sintering guide rod and the connecting sleeve are at the specified position; then, hang the optical fiber preform on the connecting sleeve; start to enter the production state, control the optical fiber preform to enter the production position, during the rod feeding process, the molybdenum heating rod is maintained at a temperature of 500℃~1100℃, and the interlayer cavity is always in an inert gas protection atmosphere. After the optical fiber preform is fed to the production position, the effective section of the optical fiber preform enters the effective position of the temperature zone and is located at the center of the temperature zone. At this time, the sintering upper sealing device forms a seal with the main furnace body furnace mouth. First, the sintering guide rod is controlled by the motor to drive the optical fiber preform to rotate at a speed of 0.5rpm~20rpm. Secondly, the interlayer chamber exhaust pneumatic valve is opened synchronously, The air pressure of the loading chamber exhaust pneumatic valve is controlled at -200Pa~-600Pa. The interlayer chamber pressure control valve and the loading chamber pressure control valve are opened simultaneously. The loading chamber pressure is set at 50Pa~2000Pa. The loading chamber pressure is monitored by the loading chamber pressure gauge, and the interlayer chamber pressure is monitored by the interlayer chamber pressure gauge to ensure that the loading chamber pressure is always greater than the interlayer chamber pressure. After maintaining for 30min~500min, the temperature is raised to the target temperature at the set slope of 0℃ / min~8℃ / min. The temperature in the main furnace is monitored in real time using an infrared thermocouple. After the temperature is raised, it is maintained for 30min~600min. After the above steps are completed, the degassing and vitrification stage is entered: First, close the interlayer chamber exhaust pneumatic valve, loading chamber exhaust pneumatic valve, and interlayer nitrogen inlet pneumatic valve, and simultaneously open the interlayer chamber vacuum pipeline pneumatic valve and loading chamber vacuum pipeline pneumatic valve, and simultaneously open the interlayer chamber vacuum pump group and loading chamber vacuum pump group, and synchronously decompress and evacuate the loading chamber and the interlayer chamber. The synchronous furnace temperature is raised to 1520℃~1560℃ at a set slope of 2℃ / min~5℃ / min to vitrify the optical fiber preform. In terms of mass percentage, the process gas is nitrogen 90%~98%, chlorine 2%~10%, and the vacuum degree of the loading chamber should be slightly lower than that of the interlayer chamber, and the control range is 0. pa~3000pa, PID control is performed through the interlayer chamber pressure control valve and the loading chamber pressure control valve. After vitrification is completed, the interlayer chamber vacuum pipeline pneumatic valve and the loading chamber vacuum pipeline pneumatic valve are closed synchronously, and the interlayer chamber vacuum pump group, the loading chamber vacuum pump group, the interlayer chamber pressure control valve, and the loading chamber pressure control valve are closed with delay. The interlayer nitrogen gas inlet pneumatic valve is opened, and the interlayer chamber air intake volume is variable, and the loading chamber air intake volume is 1L / min~5L / min. Then, the gas mass flow controller is regulated by PLC to ensure that the absolute value of the pressure difference between the loading chamber pressure gauge and the interlayer chamber pressure gauge is within 0pa~3000pa. After the pressurization is completed, the temperature is cooled synchronously to the standby temperature of 800℃, and the product is lifted to the rod hanging and taking point through the sintering guide rod and the connecting sleeve, and the production department is notified to take the rod to complete this production.
2. The method for using the low water peak optical fiber preform helium-free sintering device according to claim 1, characterized in that: The loading chamber and the interlayer chamber are separated by a silicon carbide furnace tube, the heating device is a molybdenum heating rod, and a furnace body tungsten heat insulation screen is arranged in the interlayer chamber and around the molybdenum heating rod.
3. The method for using the low water peak optical fiber preform helium-free sintering device according to claim 1, characterized in that: The loading chamber exhaust system includes a loading chamber air duct, which includes a main path and a branch path, which are respectively connected to the exhaust duct, and the main path is provided with a loading chamber pressure control valve and a loading chamber exhaust pneumatic valve, and the branch path is provided with a loading chamber vacuum pipeline pneumatic valve and a loading chamber vacuum pump group.
4. The method for using the low water peak optical fiber preform helium-free sintering device according to claim 1, characterized in that: The interlayer chamber exhaust system comprises an interlayer chamber air duct, which is connected with an exhaust duct. The interlayer chamber air duct is provided with an interlayer nitrogen gas intake pneumatic valve, an interlayer chamber pressure control valve, an interlayer chamber vacuum pipeline pneumatic valve and an interlayer chamber exhaust pneumatic valve. The interlayer nitrogen gas intake pneumatic valve is arranged between the interlayer chamber air duct and a gas mass flow controller. The interlayer chamber vacuum pipeline pneumatic valve is arranged between the interlayer chamber air duct and the interlayer chamber vacuum pump group. The interlayer chamber vacuum pump group is also connected with the exhaust duct.
5. The method for using the low water peak optical fiber preform helium-free sintering device according to claim 4, characterized in that: The exhaust duct is connected to the main air duct, and the main air duct is used to realize the function of transporting the waste gas of the interlayer cavity and the loading cavity.
6. The method for using the low water peak optical fiber preform helium-free sintering device according to claim 1, characterized in that: The optical fiber preform is connected to one end of a sintering guide rod through a connecting sleeve, and the other end of the sintering guide rod is arranged on the equipment tower. The sintering guide rod is hollow inside and communicates with the loading chamber. The sintering guide rod can realize the feeding and lifting actions of the optical fiber preform from top to bottom or from bottom to top.
7. The method for using the low water peak optical fiber preform helium-free sintering device according to claim 6, characterized in that: The loading chamber is connected to the gas mixing device through the sintering guide rod, and an upper loading air intake pneumatic valve is arranged between the sintering guide rod and the gas mixing device. The gas ratio of the loading chamber intake is regulated by the gas mixing device.
8. The method for using the low water peak optical fiber preform helium-free sintering device according to claim 6, characterized in that: The top of the main furnace body is provided with a sintering upper sealing device for achieving sealing with the sintering guide rod and sealing with the furnace mouth of the main furnace body.
9. The method for using the low water peak optical fiber preform helium-free sintering device according to claim 1, characterized in that: The main furnace body is provided with a loading chamber pressure gauge, an interlayer chamber pressure gauge and an infrared thermocouple. The loading chamber pressure gauge is communicated with the loading chamber, and real-time monitoring of the loading chamber pressure is achieved through the loading chamber pressure gauge. The interlayer chamber pressure gauge is communicated with the interlayer chamber, and real-time monitoring of the interlayer chamber pressure is achieved through the interlayer chamber pressure gauge. Real-time monitoring of the temperature inside the main furnace body is achieved through the infrared thermocouple.