TPU hot melt adhesive for high yellowing resistance and high viscosity invisible car cover and preparation method and application thereof
By preparing high yellow-resistant and high viscosity TPU hot melt adhesive, the high temperature and high viscosity problems of TPU hot melt adhesive in automotive invisible car clothing attachment are solved, and the safety and environmental protection are improved through solvent-free process, realizing the traditional Improved performance of glue.
Patent Information
- Application Number
- CN202411080228.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-08
AI Technical Summary
The high melting temperature and high viscosity of existing TPU hot melt adhesives make it difficult to apply to the attachment of car invisible car clothing, and traditional polyacrylic glues have safety hazards and environmental pollution problems.
High yellow-resistant and high viscosity TPU hot melt adhesive is prepared by raw materials such as polymer diols, isocyanates, curing agents, catalysts and plasticizers. The viscosity is reduced by adjusting the temperature and component ratio, and it is prepared and applied under solvent-free conditions.
It realizes high adhesion between TPU car coat substrate and glue, reduces operation difficulty and environmental pollution risks, and provides a safer and more environmentally friendly invisible car coat attachment solution.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thermoplastic polyurethane elastomers, and particularly relates to a TPU hot melt adhesive for a highly yellowing-resistant and highly viscous invisible car cover, and a preparation method and application thereof. Background Art
[0002] TPU-based invisible car cover is a transparent film made of polyurethane. Its chemical and physical properties are very stable, and its wear resistance is also very strong. It is an excellent material. TPU-based invisible car cover has strong toughness, wear resistance, weather resistance, and good stretchability. After installation, it can isolate the car paint from the air, prevent acid rain, oxidation, and scratches, and protect the car's paint surface for a long time. It also has higher brightness and incredible scratch repair function.
[0003] The TPU car cover film is composed of two layers of release film, a functional coating, glue, and a TPU base film, wherein the glue is currently generally a polyacrylic acid material. Patent CN109825224A discloses a hot and cold alternating removable acrylic pressure-sensitive adhesive, a preparation method, and its application, but the bonding effect between the glue of this invention and the TPU substrate is poor. Patent CN105001813A discloses a silicone-modified acrylic pressure-sensitive adhesive and a preparation method thereof, and the glue of this invention has a low peeling force. Moreover, patents CN114920870A, CN115975555A, CN115806787A, CN105001813A and other inventions all involve the use of polyacrylic acid pressure-sensitive adhesive for invisible car covers. However, this type of glue all involves solvents, which poses certain safety hazards to the environment and people during production and use.
[0004] In the prior art, there is no precedent for applying TPU hot melt adhesive to invisible car cover films. The reason is that the melting temperature of TPU hot melt adhesive is high, mostly above 100°C and below 150°C. Although it melts, it has a relatively high viscosity. Car cover attachment is a manual operation, and too high a temperature will increase the difficulty of the operation. In addition, the hot melt adhesive still maintains a high viscosity after hot melting, making it difficult to distribute the adhesive layer evenly and difficult to apply to car cover attachment. Summary of the invention
[0005] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a TPU hot melt adhesive for invisible car cover with high yellowing resistance and high viscosity, which has significantly better adhesion to TPU base film materials than polyacrylic adhesives and is safe and environmentally friendly.
[0006] The invention also provides a preparation method thereof, which is simple and feasible and suitable for large-scale production.
[0007] The invention also provides an application thereof, which can be hot-melted at a temperature greater than 90° C. into low-viscosity glue for attaching invisible car covers.
[0008] The TPU hot melt adhesive for invisible car cover with high yellowing resistance and high viscosity of the present invention is made of the following raw materials in parts by weight:
[0009] 100 parts of polymer diol;
[0010] 23.7-45.5 parts of diisocyanate;
[0011] Curing agent 1.5-10.44 parts;
[0012] Catalyst 0.5-1 part;
[0013] 3-10 parts of plasticizer;
[0014] The curing agent is a mixture of small molecule diol, small molecule dioxime and trimethylolpropane (TMP) in a molar ratio of (0-1):1:(0.01-0.1);
[0015] The diisocyanate is one of isophorone diisocyanate (IPDI), 4,4'-dicyclohexylmethane diisocyanate (HMDI), hexamethylene diisocyanate (HDI) or a mixture thereof in any proportion.
[0016] The small molecule diol is one or more of butanediol, neopentyl glycol and hexanediol.
[0017] The small molecule dioxime is one or more of 2,4-pentanedione dioxime, dimethylglyoxime, and 1,2-cyclohexanedione dioxime.
[0018] The polymer diol is a polyester diol, and the number average molecular weight of the polymer diol is 500-2000 g / mol.
[0019] The polyester diol is one or more of polycaprolactone diol, polybutylene adipate diol, polyhexane adipate diol, and polybutylene adipate diol.
[0020] The catalyst is an organic bismuth catalyst, preferably bismuth neodecanoate CB83.
[0021] The plasticizer is tributyl citrate (TBC).
[0022] The method for preparing the TPU hot melt adhesive for invisible car cover with high yellowing resistance and high viscosity of the present invention comprises the following steps:
[0023] (1) Add the polymer diol into a reaction vessel, heat to 80-130°C until it is completely melted, add the curing agent, catalyst and plasticizer, and stir;
[0024] (2) Add diisocyanate into a reaction vessel and stir to react;
[0025] (3) Pour the mixture obtained after the reaction in step (2) into a baking pan with a Teflon coating and ripen it to obtain a TPU hot melt adhesive for invisible car cover with high yellowing resistance and high viscosity.
[0026] The stirring time in step (1) is 5-12 hours, the stirring reaction time in step (2) is 10-20 hours, and the aging temperature in step (3) is 60-90° C., and the aging time is 15-24 hours.
[0027] The application of the TPU hot melt adhesive for invisible car cover with high yellowing resistance and high viscosity of the present invention is that the TPU hot melt adhesive is heated to above 90° C. and used as glue for attaching invisible car cover.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] 1) The hot melt adhesive of the present invention has a high final bonding strength due to the addition of TMP. At the same time, the hot melt adhesive of the present invention is made of thermoplastic polyurethane elastomer, and its bonding strength with the TPU car cover substrate film is significantly greater than that of conventional acrylic type glue.
[0030] 2) The present invention does not involve any solvent in the whole process, is friendly to the environment and personnel, and avoids the solvent from damaging the base film of the car cover.
[0031] 3) The present invention embeds the oxime urethane bond into the structure through dioxime. The material shows that the oxime urethane bond gradually dissociates when the temperature is greater than 90°C, and the viscosity of the material decreases accordingly. The addition of plasticizer further reduces the viscosity of the system, which facilitates the subsequent glue coating of the TPU film and the car cover film process.
[0032] 4) The use of aliphatic isocyanate ensures that the hot melt adhesive of the invention has high yellowing resistance and a lower outflow temperature. DETAILED DESCRIPTION
[0033] The present invention will be further described below with reference to the embodiments.
[0034] Unless otherwise specified, all raw materials used in the examples are commercially available.
[0035] Example 1
[0036] The raw materials and their mass fractions of the TPU hot melt adhesive for the highly yellowing-resistant and highly viscous invisible car cover are as follows:
[0037] Polycaprolactone diol (Mn=1000g / mol): 100 parts;
[0038] HMDI: 32 parts;
[0039] Curing agent (butylene glycol / dimethylglyoxime / TMP): 0 / 3 / 0.3 parts;
[0040] CB83: 1;
[0041] TBC: 3 servings;
[0042] The preparation method of the TPU hot melt adhesive for the highly yellowing-resistant and highly viscous invisible car cover:
[0043] (1) Add polycaprolactone diol into a three-necked flask, heat it at 100°C until it is completely melted, add curing agent (dimethylglyoxime / TMP), CB83, and TBC, and stir for 12 hours;
[0044] (2) Add HMDI into the flask and stir to react for 20 hours;
[0045] (3) Pour the reaction mixture into a Teflon-coated baking pan and cure it at 80°C for 24 hours to obtain a TPU hot melt adhesive for invisible car cover with high yellowing resistance and high viscosity.
[0046] Example 2
[0047] The raw materials and their mass fractions of the TPU hot melt adhesive for the highly yellowing-resistant and highly viscous invisible car cover are as follows:
[0048] Poly(hexanediol adipate) diol (Mn=2000g / mol): 100 parts;
[0049] HDI: 23.7 parts;
[0050] Curing agent (butylene glycol / dimethylglyoxime / TMP): 4.5 / 5.8 / 0.14 parts;
[0051] CB83: 0.5 parts;
[0052] TBC: 5 servings;
[0053] The preparation method of the TPU hot melt adhesive for the highly yellowing-resistant and highly viscous invisible car cover:
[0054] (1) Add poly(hexanediol adipate) diol into a three-necked flask, heat to 130°C until completely melted, add curing agent (butanediol / dimethylglyoxime / TMP), CB83, and TBC, and stir for 9 hours;
[0055] (2) Add HDI into the flask and stir to react for 15 hours;
[0056] (3) Pour the reaction mixture into a Teflon-coated baking pan and cure it at 70°C for 15 hours to obtain a TPU hot melt adhesive for invisible car cover with high yellowing resistance and high viscosity.
[0057] Example 3
[0058] The raw materials and their mass fractions of the TPU hot melt adhesive for the highly yellowing-resistant and highly viscous invisible car cover are as follows:
[0059] Polybutylene adipate diol (Mn=500g / mol): 100 parts;
[0060] IPDI: 45.5 parts;
[0061] Curing agent (hexanediol / 2,4-pentanedione dioxime / TMP): 0.45 / 1.0 / 0.05 parts;
[0062] CB83: 0.5 parts;
[0063] TBC: 10 servings;
[0064] (1) Add polybutylene adipate diol into a three-necked flask and heat to 80°C until completely melted. Add curing agent (hexanediol / 2,4-pentanedione dioxime / TMP), CB83, and TBC and stir for 5 hours.
[0065] (2) Add IPDI into the flask and stir to react for 10 hours;
[0066] (3) Pour the reaction mixture into a Teflon-coated baking pan and cure it at 60°C for 20 hours to obtain a TPU hot melt adhesive for invisible car cover with high yellowing resistance and high viscosity.
[0067] Example 4
[0068] The raw materials and their mass fractions of the TPU hot melt adhesive for the highly yellowing-resistant and highly viscous invisible car cover are as follows:
[0069] Polybutylene adipate-hexanediol ester diol (Mn=1000g / mol): 100 parts;
[0070] HMDI / HDI: 14.7 / 14.7 parts;
[0071] Curing agent (neopentyl glycol / 1,2-cyclohexanedione dioxime / TMP): 2 / 4 / 0.1 parts;
[0072] CB83: 0.75 parts;
[0073] TBC: 8 servings;
[0074] The preparation method of the TPU hot melt adhesive for the highly yellowing-resistant and highly viscous invisible car cover:
[0075] (1) Add polybutylene adipate-hexanediol diol into a three-necked flask, heat to 80°C until completely melted, add curing agent (neopentyl glycol / 1,2-cyclohexanedione dioxime / TMP), CB83, and TBC, and stir for 5 hours;
[0076] (2) Add HMDI + HDI into the flask and stir to react for 10 hours;
[0077] (3) Pour the reaction mixture into a Teflon-coated baking pan and cure it at 80°C for 20 hours to obtain a TPU hot melt adhesive for invisible car cover with high yellowing resistance and high viscosity.
[0078] Example 5
[0079] The raw materials and their mass fractions of the TPU hot melt adhesive for the highly yellowing-resistant and highly viscous invisible car cover are as follows:
[0080] Polycaprolactone diol (Mn=1500g / mol); polyhexanediol adipate diol (Mn=1500g / mol): 50 / 50 parts;
[0081] HMDI: 30 parts;
[0082] Curing agent (neopentyl glycol / dimethylglyoxime / 1,2-cyclohexanedione dioxime / TMP): 0.14 / 3.2 / 3.5 / 0.075 parts;
[0083] CB83: 0.5 parts;
[0084] TBC: 10 servings;
[0085] The preparation method of the TPU hot melt adhesive for the highly yellowing-resistant and highly viscous invisible car cover:
[0086] (1) Add polycaprolactone diol (Mn=1500 g / mol) and polyhexanediol adipate diol (Mn=1500 g / mol) into a three-necked flask, heat to 80°C until completely melted, add curing agent (neopentyl glycol / dimethylglyoxime / 1,2-cyclohexanedione dioxime / TMP), CB83, and TBC, and stir for 5 hours;
[0087] (2) Add HMDI into the flask and stir to react for 10 hours;
[0088] (3) Pour the reaction mixture into a Teflon-coated baking pan and cure it at 90°C for 24 hours to obtain a TPU hot melt adhesive for invisible car cover with high yellowing resistance and high viscosity.
[0089] Comparative Example 1
[0090] The HMDI in Example 1 was replaced with an equimolar amount of MDI to obtain the final product.
[0091] Comparative Example 2
[0092] The dimethylglyoxime in Example 2 was replaced with an equal mole of 1,4-butanediol (BDO) to obtain the final product.
[0093] The performance of the TPU hot melt adhesive for invisible car cover obtained in the embodiment and the comparative example was tested respectively, and the finished car cover adhesive Foshan Linggu Artetak-NP58 was selected for comparison, and the data is recorded in Table 1.
[0094] The specific test method is as follows:
[0095] Viscosity test, in accordance with GBT 10247-2008.
[0096] Outflow temperature was measured using a Shimadzu capillary rheometer.
[0097] Yellowing resistance test, according to ASTM-D1148, method B.
[0098] For the peel strength test, the samples were attached to the TPU material and the paint panel for car cover, hot pressed at 130℃ for 15s, cooled for 30min and 24h, cut into 25mm wide strips, the tensile rate was 100mm / min, the peeling angle was 180, and the test result was the average value of 3 parallel strips;
[0099] For the weathering test, samples were prepared according to the method for testing peel strength. Each sample was divided into two groups. One group was placed at room temperature, and the other group was placed in a UV light box at 30°C for 24 hours, a refrigerator at -18°C for 24 hours, and a constant temperature and humidity box at 85°C (humidity 85% RH) for 24 hours. This cycle was repeated 5 times in sequence. After the placement, the viscosity of the two groups of samples was tested.
[0100] Debonding: Apply a certain amount of sample between the sheets of TPU material for car cover, heat press at 130℃ for 15s, tear it apart, repeat 30 times, and check the distribution of the adhesive layer on the surface of the TPU sheet;
[0101] Smell test, experimenter's sense of smell.
[0102] Table 1 Performance of the embodiments, comparative examples and Foshan Linggu Artetak-NP58
[0103]
[0104] It can be seen from the data in Table 1 that when the glue of the present invention is heated to above 90°C, the viscosity becomes significantly smaller and is lower than that of conventional glue, which facilitates operation during the lamination of car covers. The yellowing resistance and weather resistance of the present invention are significantly better than conventional glues on the market. In terms of viscosity, the present invention is significantly better than conventional glues on the market. Compared with Comparative Example 1, the embodiment has advantages in yellowing resistance and weather resistance, and the lower viscosity and outflow temperature ensure that the hot melt adhesive is easy to operate during use.
Claims
1. A TPU hot melt adhesive for invisible car cover with high yellowing resistance and high viscosity, characterized in that: Made from the following raw materials in parts by weight: 100 parts of polymer diol; 23.7-45.5 parts of diisocyanate; Curing agent 1.5-10.44 parts; Catalyst 0.5-1 part; 3-10 parts of plasticizer; The curing agent is a mixture of small molecule diol, small molecule dioxime and trimethylolpropane in a molar ratio of (0-1):1:(0.01-0.1); the diisocyanate is one of isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, hexamethylene diisocyanate or a mixture thereof in any proportion; The plasticizer is tributyl citrate; Heat the TPU hot melt adhesive to above 90°C and use it as glue for attaching invisible car covers.
2. The TPU hot melt adhesive for invisible car cover with high yellowing resistance and high viscosity according to claim 1, characterized in that: The small molecule diol is one or more of butanediol, neopentyl glycol and hexanediol.
3. The TPU hot melt adhesive for invisible car cover with high yellowing resistance and high viscosity according to claim 1, characterized in that: The small molecule dioxime is one or more of 2,4-pentanedione dioxime, dimethylglyoxime, and 1,2-cyclohexanedione dioxime.
4. The TPU hot melt adhesive for invisible car cover with high yellowing resistance and high viscosity according to claim 1, characterized in that: The polymer diol is a polyester diol, and the number average molecular weight of the polymer diol is 500-2000 g / mol.
5. The TPU hot melt adhesive for invisible car cover with high yellowing resistance and high viscosity according to claim 4, characterized in that: The polyester diol is one or more of polycaprolactone diol, polybutylene adipate diol and polyhexane adipate diol.
6. The TPU hot melt adhesive for invisible car cover with high yellowing resistance and high viscosity according to claim 1, characterized in that: The catalyst is an organic bismuth catalyst.
7. A method for preparing the TPU hot melt adhesive for invisible car cover with high yellowing resistance and high viscosity according to any one of claims 1 to 6, characterized in that: The following steps are involved: (1) Add the polymer diol into a reaction vessel, heat until completely melted, add the curing agent, catalyst and plasticizer, and stir; (2) Add diisocyanate into a reaction vessel and stir to react; (3) The mixture after the reaction in step (2) is aged to obtain a TPU hot melt adhesive for invisible car cover with high yellowing resistance and high viscosity.
8. The method for preparing the TPU hot melt adhesive for invisible car cover with high yellowing resistance and high viscosity according to claim 7, characterized in that: The stirring time in step (1) is 5-12 hours, the stirring reaction time in step (2) is 10-20 hours, and the aging temperature in step (3) is 60-90° C., and the aging time is 15-24 hours.
9. An application of the TPU hot melt adhesive for invisible car cover with high yellowing resistance and high viscosity as claimed in any one of claims 1 to 6, characterized in that: Heat the TPU hot melt adhesive to above 90°C and use it as glue for attaching invisible car covers.
Citation Information
Cited By
Brightening aliphatic TPU base film for invisible car cover and preparation method of brightening aliphatic TPU base film
CN122011740A