A preparation method of UV light-curing magnetic adhesive
Through the preparation method of solvent-free UV photocuring magnetic glue, the polymerization of pentaerythritol tetramercaptoacetate and allyl (cyclopentadienyl) nickel was solved by combining photoinitiator to polymerize under ultraviolet light. In the prior art, solvents are flammable and explosive and have poor performance, and high-performance and environmentally friendly UV light-cured magnetic adhesive is achieved.
Patent Information
- Application Number
- CN202410826719.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-06-25
AI Technical Summary
The existing UV light curing magnetic glue contains a large amount of organic solvents, which are flammable and explosive, harmful to the human body, are not environmentally friendly, and its stickiness and 180° peel strength are not ideal.
Using a preparation method of UV photocuring magnetic glue, rosin polymerization is added by weighing isooctyl acrylate, butyl acrylate, polyurethane acrylate, 2-hydroxyethyl acrylate, synergist and photoinitiator by weight. substances, color paste, sperm, sperm acid, vapor phase silica and glass microbeads, stir and react to form solvent-free UV photocuring magnetic glue, using pentaerythritol tetramercaptoacetate and allyl (cyclopentadienyl) nickel The components are equal to form a nickel complex, and the photoinitiator is combined with a photoinitiator to perform rapid polymerization under ultraviolet light to form a crosslinking network structure.
The prepared UV light curing magnetic glue is non-toxic and non-combustible, safe and environmentally friendly, with low cost, significantly improved viscosity and 180° peel strength, excellent overall performance, and is suitable for application scenarios in different environments.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of UV light-curing magnetic adhesive preparation, in particular to a method for preparing UV light-curing magnetic adhesive. Background Art
[0002] UV light-curing magnetic adhesive is widely used in various fields such as medical care, aviation, electronics, printing, optical instruments, etc. Its advantages are 100% curing film, no solvent volatilization pollution, fast curing speed, energy saving and high production efficiency.
[0003] Chinese patent CN101928541B: A mercapto / cyanoacrylate UV curing adhesive composition, comprising 5-60% of a mercapto compound selected from mercapto alkyl esters and alkyl mercaptans; 5-60% of an α-cyanoacrylate selected from the following general formula; 0-60% of a prepolymer selected from polyester acrylate prepolymers, epoxy acrylate prepolymers, and polyurethane acrylate prepolymers; 0-50% of an active monomer selected from monofunctional, difunctional or multifunctional acrylates, allyl compounds or vinyl compounds; 1-10% of a photoinitiator and 0-10% of an auxiliary agent.
[0004] Chinese patent CN109181619A: discloses a UV light-curing magnetic adhesive, which includes the following components by weight: difunctional modified polyurethane acrylate, weight ratio 20%-70%; grafted difunctional modified polyurethane acrylate, weight ratio 5%-50%, trifunctional modified polyurethane acrylate, weight ratio 0.1%-10%; hydroxyethyl methacrylate, weight ratio 5-35%; isobornyl acrylate, weight ratio 15-45%; N-vinyl caprolactam, weight ratio 5-40%; N-vinyl pyrrolidone, weight ratio 5-40%; 1-hydroxycyclohexyl phenyl ketone, weight ratio 1-10%; 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, weight ratio 1-10%; phosphor, stabilizer and filler, weight ratio 0.1-10.0%.
[0005] Chinese patent CN118064086A: discloses a UV light-curing magnetic adhesive and a preparation method thereof, which is made of the following raw materials in parts by weight: 10-20 parts of acrylic acid-modified polyetheretherketone, 3-5 parts of bis(1-vinylimidazole-2-)ketone, 2-4 parts of 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, 1-2 parts of bis(3-aminophenyl)3,5-bis(trifluoromethyl)phenylphosphine oxide, 4-6 parts of 1,3-bis(oxiranylmethyl)-5-(2-propenyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 25-35 parts of diluent, 1-4 parts of photoinitiator, and 0.5-1 part of defoaming agent.
[0006] The UV light-curing magnetic adhesives prepared by the above patents and prior art are mostly solvent-based UV light-curing magnetic adhesives. Solvent-based UV light-curing magnetic adhesives contain a large amount of organic solvents, which are flammable, explosive, volatile, harmful to the human body, and not environmentally friendly; and the adhesive holding force and 180° peel strength are not ideal. Summary of the invention
[0007] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a method for preparing a UV light-curing magnetic adhesive.
[0008] In order to achieve the above object, the present invention adopts the following technical solutions:
[0009] A method for preparing UV light-curing magnetic adhesive, the operating steps are as follows:
[0010] S1: weigh 18-36 parts of isooctyl acrylate, 18-36 parts of butyl acrylate, 10-20 parts of polyurethane acrylate, 16-32 parts of 2-hydroxyethyl acrylate, 4-8 parts of synergist, and 1-3 parts of photoinitiator by weight, add them to a reaction kettle, stir at a rate of 200-300 rpm, and stir for 10 min-30 min;
[0011] S2 continues to add 3-7 parts of rosin polymer, 0.1-1 parts of color paste, 1-5 parts of liter acid, 5-10 parts of fumed silica, and 5-10 parts of glass beads, and reacts at 50-60° C. with stirring for 50-100 minutes to obtain UV light-curing magnetic adhesive.
[0012] As a further solution of the present invention: the photoinitiator is one of diaryl iodonium salt, triaryl iodonium salt, alkyl iodonium salt, and cumene ferrocenium hexafluorophosphate.
[0013] As a further solution of the present invention: the preparation method of the synergist is:
[0014] By weight, 21-42 parts of pentaerythritol tetrathioglycolate, 0.3-3 parts of allyl (cyclopentadienyl) nickel, CAS: 12107-46-9, 0.001-0.02 parts of allyl epoxy polyether, 0.3-3 parts of ethylenediamine, and 200-260 parts of DMF are stirred at 50-60° C. for reaction for 20-50 minutes, and the DMF is removed by distillation to obtain a synergist.
[0015] As a further solution of the present invention: the allyl epoxy polyether is selected from APE1000, APE600, and APE1500.
[0016] As a further solution of the present invention: the method for using the UV light-curing magnetic adhesive comprises: evenly coating the UV light-curing magnetic adhesive on a substrate, covering the adhesive with a layer of release film, and exposing the adhesive to ultraviolet light for irradiation and curing.
[0017] As a further solution of the present invention: the wavelength of the ultraviolet light is 180-400nm.
[0018] As a further solution of the present invention: the substrate is one of paper, plastic film, glass fiber cloth and metal film.
[0019] As a further solution of the present invention: the release film is a polypropylene film or a polyester film.
[0020] Reaction mechanism
[0021] Pentaerythritol tetrathioglycolate contains multiple active thiol groups, which undergo addition reaction with the allyl group in allyl(cyclopentadienyl)nickel to form a stable nickel complex intermediate; the nickel-containing complex obtained above is further reacted with allyl epoxy polyether; due to the high reactivity of the epoxy group, it undergoes a ring-opening reaction with the remaining thiol groups or coordinated hydrogen in the complex to form longer chain molecules, which increases the overall molecular weight and flexibility of the final polymer.
[0022] Under the action of ultraviolet light, the remaining thiol groups in the aforementioned products undergo a rapid thiol-olefin click chemistry reaction with monomers such as isooctyl acrylate and butyl acrylate; the photoinitiator decomposes in this process to produce free radicals, thereby quickly starting and completing the polymerization process to form a cross-linked network structure.
[0023] Technical Effects
[0024] The present invention discloses a method for preparing a UV light-curing magnetic adhesive. Compared with the prior art, the present invention has the following significant effects:
[0025] 1. The present invention does not add solvents, so the prepared UV light-curing magnetic adhesive is non-toxic and non-flammable, safe, environmentally friendly and low in cost;
[0026] 2. The UV light-curing magnetic adhesive prepared by the present invention has an introduced nickel complex that enhances the cohesive force between molecules through interaction with other components. At the same time, the polymer network formed by light curing has good mechanical strength. The two work together to enable the adhesive to withstand greater force when peeled off. The obtained UV light-curing magnetic adhesive has an adhesive holding force of >1000 and a 180° peel strength of 22.3N / 25mm, which can significantly improve the wettability and bonding strength, and has good comprehensive performance.
[0027] 3. Enhanced environmental adaptability: The introduction of polyether segments increases the flexibility and temperature resistance of the adhesive; this property enables the adhesive to maintain stable performance under different temperatures and usage environments, and is particularly suitable for application scenarios with large changes in the external environment. DETAILED DESCRIPTION
[0028] The following examples will help those skilled in the art to further understand the present invention, but do not limit the present invention in any form. For those of ordinary skill in the art, without departing from the inventive concept, some changes and improvements can also be made, which all belong to the protection scope of the present invention. The endpoints and any values of the ranges disclosed in this article are not limited to the precise range or value, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, between the endpoint values of each range, between the endpoint values of each range and a separate point value, and between separate point values, one or more new numerical ranges can be combined with each other, and these numerical ranges should be regarded as specifically disclosed in this article, and the present invention is described in detail below in conjunction with specific embodiments:
[0029] 1. Adhesion: Refer to GB / T4851-2014 and use CNY-2 adhesion tester to measure;
[0030] 2. 180° peel strength: refer to GB / T2792-2014 and measured by KJ-1065 series peel strength testing machine.
[0031] Example 1
[0032] A method for preparing UV light-curing magnetic adhesive, the operating steps are as follows:
[0033] S1: Weigh 18g of isooctyl acrylate, 18g of butyl acrylate, 10g of polyurethane acrylate, 16g of 2-hydroxyethyl acrylate, 4g of synergist, and 1g of photoinitiator, add them into a reactor, stir at a rate of 200 rpm, and stir for 10 min.
[0034] S2: Continue to add 3g of rosin polymer, 0.1g of color paste, 1g of fine acid, 5g of fumed silica, and 5g of glass beads, and stir at 50°C for 50 minutes to obtain UV light-curing magnetic adhesive.
[0035] The photoinitiator is a diaryl iodonium salt.
[0036] The preparation method of the synergist is:
[0037] 21g of pentaerythritol tetrathioglycolate, 0.3g of allyl (cyclopentadienyl) nickel, CAS: 12107-46-9, 0.001g of allyl epoxy polyether, 0.3g of ethylenediamine, and 200g of DMF were stirred at 50°C for 20 minutes, and the DMF was distilled off to obtain a synergist.
[0038] The allyl epoxy polyether is selected from APE1000.
[0039] The method for using the UV light-curing magnetic adhesive comprises: evenly coating the UV light-curing magnetic adhesive on a substrate, covering the adhesive with a layer of release film, and placing the adhesive under ultraviolet light for irradiation and curing.
[0040] The wavelength of the ultraviolet light is 180nm.
[0041] The substrate is paper.
[0042] The release film is a polypropylene film.
[0043] Example 2
[0044] A method for preparing UV light-curing magnetic adhesive, the operating steps are as follows:
[0045] S1: Weigh 22g of isooctyl acrylate, 24g of butyl acrylate, 13g of polyurethane acrylate, 20g of 2-hydroxyethyl acrylate, 5g of synergist, and 2g of photoinitiator, add them into a reactor, stir at a rate of 250 rpm, and stir for 15 min.
[0046] S2: Continue to add 4g of rosin polymer, 0.5g of color paste, 2g of fine acid, 6g of fumed silica, and 6g of glass beads, and stir at 55°C for 60 minutes to obtain UV light-curing magnetic adhesive.
[0047] The photoinitiator is a triaryl iodonium salt.
[0048] The preparation method of the synergist is:
[0049] 28g of pentaerythritol tetrathioglycolate, 1g of allyl (cyclopentadienyl) nickel, CAS: 12107-46-9, 0.01g of allyl epoxy polyether, 1g of ethylenediamine, and 220g of DMF were stirred at 55°C for 30 minutes, and the DMF was distilled off to obtain a synergist.
[0050] The allyl epoxy polyether is selected from APE600.
[0051] The method for using the UV light-curing magnetic adhesive comprises: evenly coating the UV light-curing magnetic adhesive on a substrate, covering the adhesive with a layer of release film, and placing the adhesive under ultraviolet light for irradiation and curing.
[0052] The wavelength of the ultraviolet light is 260nm.
[0053] The substrate is a plastic film.
[0054] The release film is a polypropylene film.
[0055] Example 3
[0056] A method for preparing UV light-curing magnetic adhesive, the operating steps are as follows:
[0057] S1: Weigh 32g of isooctyl acrylate, 30g of butyl acrylate, 18g of polyurethane acrylate, 28g of 2-hydroxyethyl acrylate, 7g of synergist, and 2g of photoinitiator, add them into a reactor, stir at a rate of 250 rpm, and stir for 25 min.
[0058] S2: Continue to add 6g of rosin polymer, 0.8g of color paste, 4g of fine acid, 8g of fumed silica, and 8g of glass beads, and stir at 55°C for 90 minutes to obtain UV light-curing magnetic adhesive.
[0059] The photoinitiator is an alkyl iodonium salt.
[0060] The preparation method of the synergist is:
[0061] 38g of pentaerythritol tetrathioglycolate, 2g of allyl(cyclopentadienyl)nickel, CAS: 12107-46-9, 0.015g of allyl epoxy polyether, 2g of ethylenediamine, and 240g of DMF were stirred at 55°C for 40 minutes, and the DMF was distilled off to obtain a synergist.
[0062] The allyl epoxy polyether is selected from APE600.
[0063] The method for using the UV light-curing magnetic adhesive comprises: evenly coating the UV light-curing magnetic adhesive on a substrate, covering the adhesive with a layer of release film, and placing the adhesive under ultraviolet light for irradiation and curing.
[0064] The wavelength of the ultraviolet light is 320nm.
[0065] The base material is glass fiber cloth.
[0066] The release film is a polyester film.
[0067] Example 4
[0068] A method for preparing UV light-curing magnetic adhesive, the operating steps are as follows:
[0069] S1: Weigh 36g of isooctyl acrylate, 36g of butyl acrylate, 20g of polyurethane acrylate, 32g of 2-hydroxyethyl acrylate, 8g of synergist, and 3g of photoinitiator, add them into a reactor, stir at a rate of 300 rpm, and stir for 30 min.
[0070] S2: Continue to add 7g of rosin polymer, 1g of color paste, 5g of fine acid, 10g of fumed silica, and 10g of glass beads, and stir at 60°C for 100 minutes to obtain UV light-curing magnetic adhesive.
[0071] The photoinitiator is cumene ferrocenium hexafluorophosphate.
[0072] The preparation method of the synergist is:
[0073] 42g of pentaerythritol tetrathioglycolate, 3g of allyl(cyclopentadienyl)nickel, CAS: 12107-46-9, 0.02g of allyl epoxy polyether, 3g of ethylenediamine, and 260g of DMF were stirred at 60°C for 50 minutes, and the DMF was removed by distillation to obtain a synergist.
[0074] The allyl epoxy polyether is selected from APE1500.
[0075] The method for using the UV light-curing magnetic adhesive comprises: evenly coating the UV light-curing magnetic adhesive on a substrate, covering the adhesive with a layer of release film, and placing the adhesive under ultraviolet light for irradiation and curing.
[0076] The wavelength of the ultraviolet light is 400nm.
[0077] The substrate is a metal film.
[0078] The release film is a polyester film.
[0079] Comparative Example 1
[0080] This example is the same as Example 1 except that no synergist is added.
[0081] Comparative Example 2
[0082] This example is the same as Example 1 except that allyl(cyclopentadienyl)nickel is not added.
[0083] Comparative Example 3
[0084] This example is the same as Example 1 except that allyl epoxy polyether is not added.
[0085] Table 1-4 and comparative examples 1-3 test results
[0086] Holding force / h 180° peel strength / N / 25mm Example 1 >1000 20.8 Example 2 >1000 21.1 Example 3 >1000 21.9 Example 4 >1000 22.3 Comparative Example 1 476 8.9 Comparative Example 2 607 13.5 Comparative Example 3 663 14.2
[0087] Through the data analysis of the above embodiments and comparative examples, the UV light-curing magnetic adhesive obtained by the present invention has an adhesion force greater than 1000 and a 180° peel strength of 22.3N / 25mm, which can significantly improve the wettability and bonding strength, and has good comprehensive performance.
[0088] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a UV light-curing magnetic adhesive, the operating steps of which are: S1: weigh 18-36 parts of isooctyl acrylate, 18-36 parts of butyl acrylate, 10-20 parts of polyurethane acrylate, 16-32 parts of 2-hydroxyethyl acrylate, 4-8 parts of synergist, and 1-3 parts of photoinitiator by weight, add them to a reaction kettle, stir at a rate of 200-300 rpm, and stir for 10 min-30 min; S2 continues to add 3-7 parts of rosin polymer, 0.1-1 parts of color paste, 1-5 parts of liter acid, 5-10 parts of fumed silica, and 5-10 parts of glass beads, and reacts at 50-60°C with stirring for 50-100 minutes to obtain UV light-curing magnetic adhesive; The preparation method of the synergist comprises the following steps: by weight, adding 21-42 parts of pentaerythritol tetrathioglycolate, 0.3-3 parts of allyl (cyclopentadienyl) nickel, 0.001-0.02 parts of allyl epoxy polyether, 0.3-3 parts of ethylenediamine and 200-260 parts of DMF, stirring and reacting at 50-60° C. for 20-50 minutes, and removing the DMF by distillation to obtain the synergist.
2. The method for preparing a UV light-curing magnetic adhesive according to claim 1, characterized in that: The photoinitiator is one of diaryl iodonium salt, triaryl iodonium salt, alkyl iodonium salt and cumene ferrocenium hexafluorophosphate.
3. The method for preparing a UV light-curing magnetic adhesive according to claim 1, characterized in that: The allyl epoxy polyether is selected from one of APE1000, APE600 and APE1500.
4. The method for using the UV light-curing magnetic adhesive according to any one of claims 1 to 3, characterized in that include: The UV light-curing magnetic adhesive is evenly coated on the substrate, and a release film is covered on the adhesive, and then irradiated under ultraviolet light for curing.
5. The method for using the UV light-curing magnetic adhesive according to claim 4, characterized in that: The wavelength of the ultraviolet light is 180-400nm.
6. The method for using the UV light-curing magnetic adhesive according to claim 4, characterized in that: The substrate is one of paper, plastic film, glass fiber cloth and metal film.
7. The method for using the UV light-curing magnetic adhesive according to claim 4, characterized in that: The release film is a polypropylene film or a polyester film.