An aluminum alloy powder for additive manufacturing and its preparation method

By preparing aluminum-silicon-carbon composite powder under an argon atmosphere and adding aluminum alloy melt, the problem of degradation of mechanical properties of aluminum alloy powder after graphene is solved, the density and mechanical properties of aluminum alloy powder are improved, and more efficient is achieved energy utilization.

CN118616724BActive Publication Date: 2024-11-15JIANGSU VILORY ADVANCED MATERIALS TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411109835.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-15
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

After adding graphene to traditional aluminum alloy powder, the mechanical properties of the molded parts will be reduced, and the energy utilization rate is low during laser molding, resulting in serious waste of resources.

Method used

The anode rod was prepared by pressing the graphite powder, silicon powder and aluminum powder under an argon atmosphere, and the aluminum silicon carbon composite powder was prepared by arc discharge method, and added it to the aluminum alloy melt, and it was broken into spherical aluminum by aerosolization method. The alloy powder is then sieved and dried to obtain an aluminum alloy powder for additive manufacturing.

Benefits of technology

The density and mechanical properties of aluminum alloy powder are improved, the bonding strength between graphene and Al is enhanced, the mechanical properties of molded parts are improved, and the energy utilization rate is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention relates to the field of additive manufacturing technology, and specifically to an aluminum alloy powder for additive manufacturing and a preparation method thereof. The aluminum alloy powder for additive manufacturing of the present invention is prepared by preparing a composite powder from graphite powder, silicon powder and aluminum powder by an arc discharge method, and then mixing the composite powder with an aluminum alloy melt, and then screening and drying after atomization treatment. The aluminum alloy powder for additive manufacturing of the present invention avoids the problem of poor compatibility between graphene and an aluminum alloy matrix, and the powder has high sphericity and high fluidity. At the same time, the reflectivity of the aluminum alloy powder is reduced, and the molded parts obtained by printing have excellent density and good mechanical properties, and have good application prospects in the field of aluminum alloy powder additive manufacturing technology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of additive manufacturing, and in particular to an aluminum alloy powder for additive manufacturing and a preparation method thereof. Background Art

[0002] Additive manufacturing (AM), also known as 3D printing technology, is different from traditional subtractive manufacturing processes. It is a process method based on the layer-by-layer stacking of materials and is widely used in the fields of automobiles, aerospace, biomedicine, electronic devices, and construction. Laser additive manufacturing (LAM), also known as laser 3D printing technology, based on laser as a heat source, is suitable for the forming and manufacturing of metals, alloys, and metal-based composite materials. At present, there are three main LAM technologies used in the forming and manufacturing of metal components: laser metal deposition (LMD) based on synchronous powder feeding of nozzles; selective laser sintering (SLS) and selective laser melting (SLM) based on automatic powder bed spreading.

[0003] As a lightweight and high-strength material, aluminum alloy has always played a pivotal role in various fields due to its excellent specific strength. Especially in the field of aerospace, the requirements for aluminum alloy are increasing and becoming increasingly demanding. In addition to requiring lightweight materials, there are also demands for flexible and integrated component design. When aluminum alloy powder is used in additive manufacturing, it is necessary to meet the requirements of lightweight and high-strength materials as well as the design and molding requirements of complex components.

[0004] Patent technical document CN202210461018.6 discloses an aluminum alloy powder material, preparation method and application for aviation additive manufacturing. The aluminum alloy powder material described in the method includes Mg: 4.5-6.5wt%, Sc: 1.0-1.5wt%, Zr: 0.5-0.8wt%, Mn: 0.7-1.2wt% by mass percentage, and the balance is Al. Compared with ordinary aluminum alloy powder materials, the aluminum alloy powder material in the present invention can break through the material solid solution limit during material forming and realize additive manufacturing. The interaction of the main elements in the material produces a large number of dispersed and fine primary phases, which inhibits the recrystallization of the structure. As the heat treatment proceeds, the secondary phase precipitates in the matrix to further improve the material strength and can be used for fuselage structural parts. However, it ignores the fact that the aluminum alloy powder has a high reflectivity to the laser during laser forming, resulting in reduced energy utilization and a large amount of waste of resources.

[0005] Patent technical document CN202110326568.2 discloses an aluminum alloy powder for additive manufacturing, a preparation method and an application thereof. The method uses a small amount of graphene powder, zirconium oxide powder and aluminum alloy powder to mix. The zirconium oxide powder mixing can prevent the agglomeration of graphene, improve the powder fluidity, improve the quality of the composite powder, hinder the crack propagation in the matrix, and produce phase toughening. Although the reflectivity of the aluminum alloy powder is reduced, due to the poor compatibility of graphene and aluminum alloy itself, it will affect the mechanical properties of the molded parts. Summary of the invention

[0006] In view of this, the purpose of the present invention is to provide an aluminum alloy powder for additive manufacturing and a preparation method thereof, so as to solve the problem that the mechanical properties of the molded parts will decrease after adding graphene to the traditional aluminum alloy powder.

[0007] Based on the above purpose, the present invention provides a method for preparing aluminum alloy powder for additive manufacturing, comprising the following steps:

[0008] S1. In an argon atmosphere, graphite powder, silicon powder and aluminum powder were prepared into an anode rod by a pressing method, and then the anode rod was prepared by an arc discharge method to prepare an aluminum-silicon-carbon composite powder;

[0009] S2..In an argon atmosphere, the aluminum alloy ingot is melted at 900°C-1000°C to form an aluminum alloy liquid, stirred evenly, cooled to 700-800°C, and aluminum-silicon-carbon composite powder is added, stirred evenly, to obtain a composite alloy melt;

[0010] S3. The composite alloy melt is led out through a flow guide tube, broken into fine droplets by gas atomization, and spherical aluminum alloy powder is obtained after solidification;

[0011] S4. Under an argon atmosphere, the spherical aluminum alloy powder is sieved and dried to obtain an aluminum alloy powder for additive manufacturing;

[0012] In the step S1, the weight ratio of graphite powder, silicon powder and aluminum powder is 10-20:0.5-1.5:10-20.

[0013] Preferably, the graphite powder in step S1 is ground through a 100-150 mesh sieve before use, the average particle size of the nano silicon powder is 20-60 nm, and the average particle size of the aluminum powder is 5-11 μm.

[0014] Preferably, the specific steps of the pressing method are: mixing graphite powder with silicon powder and aluminum powder and grinding them for 2-4 hours, vacuum drying, and then transferring them to a mold, and hot pressing them at 2-3 MPa and 450-500° C. to form an anode rod with a diameter of 8-10 mm.

[0015] Preferably, the atmosphere of the arc discharge method in step S1 is a mixed gas of nitrogen and ammonia in a volume ratio of 10:1, the anode is an anode rod, the cathode is a pure graphite rod with a diameter of 15-20 mm, the inlet temperature is 400-450°C, the discharge voltage is 30-38V, the discharge current is 45-60A, and the discharge time is 40s.

[0016] Preferably, the aluminum alloy ingot is one of AlSi10Mg, AlSi7Mg, and AlSi12.

[0017] Preferably, in step S2, the weight ratio of the aluminum alloy ingot to the aluminum silicon carbon composite powder is 100-150:5-10.

[0018] Preferably, the guide tube in step S3 is made of zirconium oxide and has an inner diameter of 4 mm to 6 mm.

[0019] Preferably, the gas flow of the atomization method in step S3 is high-pressure nitrogen with a pressure of 8MPa-10MPa and a speed of 300-700 m / s.

[0020] Preferably, the aluminum alloy powder for additive manufacturing in step S4 has a particle size distribution of 15-70 μm and an average particle size of 35-40 μm.

[0021] Preferably, the drying temperature in step S4 is 55-115° C., the vacuum degree is ≤1000 Pa, and the drying time is 6-8 h.

[0022] Furthermore, the present invention also provides an aluminum alloy powder for additive manufacturing, and the aluminum alloy powder for additive manufacturing is prepared by the above-mentioned method for preparing the aluminum alloy powder for additive manufacturing.

[0023] Beneficial effects of the present invention:

[0024] (1) The aluminum alloy powder for additive manufacturing of the present invention is prepared by mixing silicon powder, graphene and aluminum powder by arc discharge method to obtain a composite powder, and then adding the composite powder to aluminum alloy melt. The density and mechanical properties of the obtained aluminum alloy powder are improved after printing.

[0025] (2) The introduction of silicon powder into the aluminum alloy powder for additive manufacturing of the present invention helps to form SiC and AlSi alloys, which can effectively improve the bonding strength between graphene and Al in the composite powder, thereby improving the mechanical properties of the molded parts. DETAILED DESCRIPTION

[0026] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0027] Example 1: An aluminum alloy powder for additive manufacturing, the specific preparation method is as follows:

[0028] (1) Grinding and sieving graphene to obtain 100-mesh graphite powder;

[0029] (2) In an argon atmosphere, 10 g of 100-mesh graphite powder, 0.5 g of silicon powder and 10 g of aluminum powder were mixed and ground for 2 h, vacuum dried, and then transferred to a mold and hot pressed at 2 MPa and 450 °C into an anode rod with a diameter of 8 mm. Subsequently, the anode rod was used as the anode and a pure graphite rod with a diameter of 15 mm was used as the cathode. The inlet temperature was 400 °C, the discharge voltage was 30 V, the discharge current was 45 A, and the discharge time was 40 s. The atmosphere of the arc discharge method was a mixed gas of nitrogen and ammonia in a volume ratio of 10:1 to obtain an aluminum-silicon-carbon composite powder;

[0030] (3) In an argon atmosphere, 100 g of AlSi10Mg alloy ingot was melted at 900 °C to form an aluminum alloy liquid. After stirring evenly, the temperature was lowered to 700 °C, 5 g of aluminum-silicon-carbon composite powder was added, and after stirring evenly, a composite alloy melt was obtained.

[0031] (4) The composite alloy melt is discharged through a zirconia flow guide tube with an inner diameter of 4 mm, and is broken into fine droplets by a gas atomization method, and spherical aluminum alloy powder is obtained after solidification; wherein the gas flow of the gas atomization method is high-pressure nitrogen with a pressure of 8 MPa and a speed of 300 m / s;

[0032] (5) Under an argon atmosphere, the spherical aluminum alloy powder is sieved and dried to obtain an aluminum alloy powder for additive manufacturing with an average particle size of 35-40 μm, wherein the drying temperature is 55° C., the vacuum degree is ≤1000 Pa, and the drying time is 6 h.

[0033] Example 2: An aluminum alloy powder for additive manufacturing, the specific preparation method is as follows:

[0034] (1) Grinding and sieving graphene to obtain 130-mesh graphite powder;

[0035] (2) In an argon atmosphere, 15 g of 130 mesh graphite powder, 1 g of silicon powder and 15 g of aluminum powder were mixed and ground for 3 h, vacuum dried, and then transferred to a mold and hot pressed at 3 MPa and 480 ° C into an anode rod with a diameter of 9 mm. Subsequently, the anode rod was used as the anode and a pure graphite rod with a diameter of 18 mm was used as the cathode. The inlet temperature was 430 ° C, the discharge voltage was 35 V, the discharge current was 47 A, and the discharge time was 40 s. The atmosphere of the arc discharge method was a mixed gas of nitrogen and ammonia in a volume ratio of 10:1 to obtain an aluminum-silicon-carbon composite powder;

[0036] (3) Under an argon atmosphere, 130 g of AlSi10Mg alloy ingot was melted at 950 °C to form an aluminum alloy liquid. After stirring evenly, the temperature was lowered to 750 °C, 8 g of aluminum-silicon-carbon composite powder was added, and after stirring evenly, a composite alloy melt was obtained;

[0037] (4) The composite alloy melt is discharged through a zirconia flow guide tube with an inner diameter of 5 mm, and is broken into fine droplets by a gas atomization method. After solidification, spherical aluminum alloy powder is obtained; wherein the gas flow of the gas atomization method is high-pressure nitrogen with a pressure of 9 MPa and a speed of 500 m / s;

[0038] (5) Under an argon atmosphere, the spherical aluminum alloy powder is sieved and dried to obtain an aluminum alloy powder for additive manufacturing with an average particle size of 35-40 μm, wherein the drying temperature is 85° C., the vacuum degree is ≤1000 Pa, and the drying time is 7 h.

[0039] Embodiment 3: An aluminum alloy powder for additive manufacturing, the specific preparation method is as follows:

[0040] (1) Grinding and sieving graphene to obtain 150-mesh graphite powder;

[0041] (2) Under an argon atmosphere, 20 g of 150 mesh graphite powder, 1.5 g of silicon powder and 20 g of aluminum powder were mixed and ground for 4 h, vacuum dried, and then transferred to a mold and hot pressed at 3 MPa and 500 ° C into an anode rod with a diameter of 8-10 mm. Subsequently, the anode rod was used as the anode and a pure graphite rod with a diameter of 20 mm was used as the cathode. The inlet temperature was 450 ° C, the discharge voltage was 38 V, the discharge current was 60 A, and the discharge time was 40 s. The atmosphere of the arc discharge method was a mixed gas of nitrogen and ammonia in a volume ratio of 10:1 to obtain an aluminum-silicon-carbon composite powder;

[0042] (3) In an argon atmosphere, 150 g of AlSi10Mg alloy ingot was melted at 1000 °C to form an aluminum alloy liquid. After stirring evenly, the temperature was lowered to 800 °C, 10 g of aluminum-silicon-carbon composite powder was added, and after stirring evenly, a composite alloy melt was obtained;

[0043] (4) The composite alloy melt is discharged through a zirconia flow guide tube with an inner diameter of 6 mm, and is broken into fine droplets by a gas atomization method. After solidification, spherical aluminum alloy powder is obtained; wherein the gas flow of the gas atomization method is high-pressure nitrogen with a pressure of 10 MPa and a speed of 700 m / s;

[0044] (5) Under an argon atmosphere, the spherical aluminum alloy powder is sieved and dried to obtain an aluminum alloy powder for additive manufacturing with an average particle size of 35-40 μm, wherein the drying temperature is 115° C., the vacuum degree is ≤1000 Pa, and the drying time is 8 h.

[0045] Comparative Example 1: An aluminum alloy powder, the specific preparation method is as follows:

[0046] (1) Grinding and sieving graphene to obtain 130-mesh graphite powder;

[0047] (2) Under an argon atmosphere, 130 g of AlSi10Mg alloy ingot was melted at 950 °C to form aluminum alloy liquid. After stirring evenly, the temperature was lowered to 750 °C, 3.85 g of 130 mesh graphite powder, 0.3 g of silicon powder and 3.85 g of aluminum powder were added, and after stirring evenly, a composite alloy melt was obtained;

[0048] (3) The composite alloy melt is discharged through a zirconia flow guide tube with an inner diameter of 5 mm, and is broken into fine droplets by a gas atomization method. After solidification, spherical aluminum alloy powder is obtained; wherein the gas flow of the gas atomization method is high-pressure nitrogen with a pressure of 9 MPa and a speed of 500 m / s;

[0049] (4) Under an argon atmosphere, the spherical aluminum alloy powder is sieved and dried to obtain an aluminum alloy powder for additive manufacturing with an average particle size of 35-40 μm, wherein the drying temperature is 85° C., the vacuum degree is ≤1000 Pa, and the drying time is 7 h.

[0050] Comparative Example 2: An aluminum alloy powder, the specific preparation method is as follows:

[0051] (1) Grinding and sieving graphene to obtain 130-mesh graphite powder;

[0052] (2) In an argon atmosphere, 15 g of 130 mesh graphite powder and 15 g of aluminum powder were mixed and ground for 3 h, vacuum dried, and then transferred to a mold and hot pressed at 3 MPa and 480 ° C to form an anode rod with a diameter of 9 mm. Subsequently, the anode rod was used as the anode and a pure graphite rod with a diameter of 18 mm was used as the cathode. The inlet temperature was 430 ° C, the discharge voltage was 35 V, the discharge current was 47 A, and the discharge time was 40 s. The atmosphere of the arc discharge method was a mixed gas of nitrogen and ammonia in a volume ratio of 10:1 to obtain an aluminum-carbon composite powder;

[0053] (3) Under an argon atmosphere, 130 g of AlSi10Mg alloy ingot was melted at 950 °C to form an aluminum alloy liquid. After stirring evenly, the temperature was lowered to 750 °C, 8 g of aluminum-carbon composite powder was added, and after stirring evenly, a composite alloy melt was obtained;

[0054] (4) The composite alloy melt is discharged through a zirconia flow guide tube with an inner diameter of 5 mm, and is broken into fine droplets by a gas atomization method. After solidification, spherical aluminum alloy powder is obtained; wherein the gas flow of the gas atomization method is high-pressure nitrogen with a pressure of 9 MPa and a speed of 500 m / s;

[0055] (5) Under an argon atmosphere, the spherical aluminum alloy powder is sieved and dried to obtain an aluminum alloy powder for additive manufacturing with an average particle size of 35-40 μm, wherein the drying temperature is 85° C., the vacuum degree is ≤1000 Pa, and the drying time is 7 h.

[0056] Comparative Example 3: An aluminum alloy powder, the specific preparation method is as follows:

[0057] (1) Grinding and sieving graphene to obtain 130-mesh graphite powder;

[0058] (2) In an argon atmosphere, 15 g of 130 mesh graphite powder, 1 g of silicon powder and 15 g of aluminum powder were mixed and ground for 3 h, vacuum dried, and then transferred to a mold and hot pressed into an anode rod with a diameter of 9 mm at 3 MPa and 480 ° C. Subsequently, the anode rod was used as the anode and a pure graphite rod with a diameter of 18 mm was used as the cathode. The inlet temperature was 430 ° C, the discharge voltage was 35 V, the discharge current was 47 A, the discharge time was 40 s, and the atmosphere of the arc discharge method was nitrogen to obtain an aluminum-silicon-carbon composite powder;

[0059] (3) Under an argon atmosphere, 130 g of AlSi10Mg alloy ingot was melted at 950 °C to form an aluminum alloy liquid. After stirring evenly, the temperature was lowered to 750 °C, 8 g of aluminum-silicon-carbon composite powder was added, and after stirring evenly, a composite alloy melt was obtained;

[0060] (4) The composite alloy melt is discharged through a zirconia flow guide tube with an inner diameter of 5 mm, and is broken into fine droplets by a gas atomization method. After solidification, spherical aluminum alloy powder is obtained; wherein the gas flow of the gas atomization method is high-pressure nitrogen with a pressure of 9 MPa and a speed of 500 m / s;

[0061] (5) Under an argon atmosphere, the spherical aluminum alloy powder is sieved and dried to obtain an aluminum alloy powder for additive manufacturing with an average particle size of 35-40 μm, wherein the drying temperature is 85° C., the vacuum degree is ≤1000 Pa, and the drying time is 7 h.

[0062] Performance Testing

[0063] Sphericity: The powders obtained in the examples and comparative examples were tested according to GB / T16418-2008. The test results are shown in Table 1.

[0064] The powders obtained in the embodiments and comparative examples were subjected to SLM printing by additive manufacturing equipment to obtain powder printed parts. The preheating temperature of the printer plate was 130°C, the laser power was 300W, the scanning speed was 1050mm / s, the scanning spacing was 0.12mm, the scanning layer thickness was 0.03mm, and the area overlap was set to 0.15mm. When the powder printed parts were annealed, the powder printed parts were heated to 325°C in a vacuum environment and kept warm for 4h, and then cooled to room temperature in air to obtain the sample powder blocks obtained in the embodiments and comparative examples. The blocks were subjected to performance tests. The test results are shown in Table 1. The specific tests are as follows:

[0065] Density: According to the Archimedean principle, the real density of the block sample is measured, and the theoretical density of the composite material is calculated. The ratio of the real density to the theoretical density is the density of the block. The density (D) calculation formula is as follows:

[0066] ;

[0067] Among them, dt: theoretical density, de: true density, D: compactness.

[0068] Microhardness:

[0069] The microhardness of the alloy was tested using a micro Vickers hardness tester (200HVS-5) with a load of 1Kg and a load loading time of 15s. The hardness of the scanning surface (xoy) and the construction surface (yoz) of the alloy was tested respectively. Before the test, the test surface of the sample was first polished with 240# to 2000# sandpaper, and then polished under a polishing machine. During the test, the hardness of at least 7 points at different positions on the observation surface was measured on each test surface. The test should avoid defects and take the average value of the measured hardness data to ensure the accuracy of the test results;

[0070] Tensile Strength:

[0071] The sample powder blocks obtained in the embodiment and the comparative example were tested using a universal testing machine (UTM500) at a tensile speed of 1.2 mm / min. The tensile specimens were cut using an electric spark wire cutting machine. After cutting the standard tensile specimens, the wire cutting marks on the surface of the specimens were polished with sandpaper to prevent affecting the test results.

[0072]

[0073] Data Analysis:

[0074] It can be seen from Examples 1-3 that the aluminum alloy powder for additive manufacturing of the present invention has excellent sphericity, which can make the powder have high fluidity, and the block density after SLM printing is not less than 99.75%; the mechanical properties are good, and the microhardness can reach 173.46HV 0.2 The tensile strength can reach 489.9MPa, and it has broad application prospects in aluminum alloy powder additive manufacturing.

[0075] It can be seen from Example 2 and Comparative Examples 1-3 that the aluminum alloy powder for additive manufacturing of the present invention, by using silicon powder as a raw material, preparing a composite powder by an arc discharge method with graphene and aluminum powder, and adding the composite powder to an aluminum alloy melt, can greatly improve the density and mechanical properties of the SLM-printed block. This may be because the addition of silicon powder can solve the problems of easy agglomeration of carbon-based reinforcement phases such as graphene and poor liquid phase wettability, and can also enhance the compatibility and bonding strength between graphene and aluminum powder, thereby improving the mechanical properties of the material.

[0076] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.

Claims

1. A method for preparing aluminum alloy powder for additive manufacturing, characterized in that: The following steps are involved: S1. In an argon atmosphere, graphite powder, silicon powder and aluminum powder were prepared into an anode rod by a pressing method, and then the anode rod was prepared by an arc discharge method to prepare an aluminum-silicon-carbon composite powder; S2. In an argon atmosphere, the aluminum alloy ingot is melted at 900 ℃-1000 ℃ into an aluminum alloy liquid, stirred evenly, cooled to 700-800 ℃, and the aluminum-silicon-carbon composite powder is added and stirred evenly to obtain a composite alloy melt; S3. The composite alloy melt is led out through a flow guide tube, broken into fine droplets by gas atomization, and spherical aluminum alloy powder is obtained after solidification; S4. Under an argon atmosphere, the spherical aluminum alloy powder is sieved and dried to obtain an aluminum alloy powder for additive manufacturing; The weight ratio of graphite powder, silicon powder and aluminum powder in step S1 is 10-20: 0.5-1.5:10-20; The atmosphere of the arc discharge method in step S1 is a mixed gas of nitrogen and ammonia in a volume ratio of 10:1, the anode is an anode rod, the cathode is a pure graphite rod with a diameter of 15-20 mm, the inlet temperature is 400-450° C., the discharge voltage is 30-38 V, the discharge current is 45-60 A, and the discharge time is 40 s.

2. The method for preparing aluminum alloy powder for additive manufacturing according to claim 1, characterized in that: The graphite powder in step S1 is ground through a 100-150 mesh sieve before use, the average particle size of the nano silicon powder is 20-60 nm, and the average particle size of the aluminum powder is 5-11 μm.

3. The method for preparing aluminum alloy powder for additive manufacturing according to claim 1, characterized in that: The specific steps of the pressing method are: mixing graphite powder, silicon powder and aluminum powder and grinding them for 2-4 hours, vacuum drying, transferring them to a mold, and hot pressing them at 2-3MPa and 450-500°C into an anode rod with a diameter of 8-10mm.

4. The method for preparing aluminum alloy powder for additive manufacturing according to claim 1, characterized in that: The aluminum alloy ingot is one of AlSi10Mg, AlSi7Mg and AlSi12.

5. The method for preparing aluminum alloy powder for additive manufacturing according to claim 1, characterized in that: The weight ratio of the aluminum alloy ingot to the aluminum silicon carbon composite powder in step S2 is 100-150:5-10.

6. The method for preparing aluminum alloy powder for additive manufacturing according to claim 1, characterized in that: The guide tube in step S3 is made of zirconium oxide and has an inner diameter of 4 mm to 6 mm.

7. The method for preparing aluminum alloy powder for additive manufacturing according to claim 1, characterized in that: The gas flow of the atomization method in step S3 is high-pressure nitrogen with a pressure of 8MPa-10MPa and a speed of 300-700 m / s.

8. The method for preparing aluminum alloy powder for additive manufacturing according to claim 1, characterized in that: The particle size distribution of the aluminum alloy powder for additive manufacturing in step S4 is 15-70 μm, and the average particle size is 35-40 μm.

9. An aluminum alloy powder for additive manufacturing, characterized in that: The aluminum alloy powder for additive manufacturing is prepared by the method for preparing the aluminum alloy powder for additive manufacturing according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Aluminum alloy powder material for aviation additive manufacturing, preparation method and application

    CN114737093A

  • Rare earth aluminum alloy powder suitable for additive manufacturing and preparation method of rare earth aluminum alloy powder

    CN112831694A

  • Aluminum alloy powder for additive manufacturing and preparation method and application thereof

    CN113084152A

  • Preparation method of graphene and silicon carbide hybrid reinforced aluminum-based composite material

    CN114951664A

  • Graphene reinforced aluminum-based composite powder, preparation method and graphene reinforced aluminum-based composite material

    CN116921678A