Glass fiber needle felt and preparation method thereof

By pretreating glass fibers and combining them with modified silica particles to form a cross-linked network structure, the strength and air permeability problems of glass fiber needle-punched felt in high-temperature corrosive environments are solved, and the high strength and corrosion resistance are improved.

CN118617818BActive Publication Date: 2024-11-08WEIFANG YOUXIN COMPOSITE MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411052739.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-08
Estimated Expiration
2044-08-02

AI Technical Summary

Technical Problem

Existing fiberglass needle-punched felt exhibits reduced strength, insufficient air permeability, and inadequate corrosion resistance under high-temperature and corrosive environments.

Method used

Glass fibers are pretreated using a specific method, combining modified silica particles and impregnation technology. The glass fibers are treated with chemical reagents such as sodium octadecyl sulfate, polyethylene glycol 200, and γ-aminopropyltriethoxysilane. Subsequently, the glass fibers react with modified silica particles, oleamide, and dodecylhydroxyethyldimethylammonium chloride to form a cross-linked network structure.

Benefits of technology

It improves the air permeability and strength of glass fiber needle-punched felt, enhances its resistance to high-temperature corrosion, and ensures stability and strength in high-temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides a glass fiber needle felt and a preparation method thereof, belonging to the technical field of glass fiber needle felt; the preparation method comprises glass fiber pretreatment, preparation of primary glass fiber needle felt and a finishing step; the finishing step comprises preparation of silicon dioxide particles, preparation of modified silicon dioxide particles and an impregnation step; the impregnation step comprises placing the primary glass fiber needle felt in an ethanol solution, adding modified silicon dioxide particles, oleic acid amide and dodecyl hydroxyethyl dimethyl ammonium chloride, heating to 61-66°C at a rate of 1.8-2.2°C / min, standing for 35-40min, and drying after standing to obtain the glass fiber needle felt; the glass fiber needle felt obtained by the invention improves air permeability while ensuring strength performance and has excellent high temperature corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of glass fiber needle felt, and in particular relates to a glass fiber needle felt and a preparation method thereof. Background Art

[0002] Glass fiber is an inorganic non-metallic material with excellent performance. It is made of six kinds of minerals, namely pyrophyllite, quartz sand, limestone, dolomite, colemanite and magnesia stone, through high-temperature melting, wire drawing, yarn winding and weaving. It has the advantages of good insulation, strong heat resistance and high mechanical strength. It is usually used as reinforcing material in composite materials, electrical insulation material, thermal insulation material, circuit substrate and other fields.

[0003] Glass fiber needle felt is a high-efficiency filter material composed of a glass fiber chopped strand felt layer and a base cloth, which are firmly combined together through needle punching and chemical bonding.

[0004] The prior art mainly discloses the following contents regarding glass fiber needle felt:

[0005] CN116065300A discloses a glass fiber needle felt and a preparation method thereof, and specifically discloses that the preparation method of the glass fiber needle felt is to acid-leach and wash the glass fiber to obtain wet base fiber, cut the wet base fiber into short fibers, dry and then loosen, card into a web, and needle-punch to obtain the needle felt, and place the needle felt on a base material and sinter it together to obtain the glass fiber needle felt;

[0006] The patented method for preparing glass fiber needle felt is highly efficient, causes little damage to the fibers, and the prepared glass fiber needle felt has high strength and a high yield rate; however, the patented glass fiber needle felt has poor high temperature resistance and corrosion resistance. In a high temperature corrosive environment, the strength of the glass fiber needle felt is greatly reduced, shortening its service life.

[0007] CN105879494A discloses a method for preparing a high-temperature resistant filter felt, which discloses that the preparation method comprises the following steps: subjecting glass fibers to an acid treatment and sintering process, and obtaining a high-silica glass fiber needle-punched felt through a combing, web-forming and needle-punching process, and then compounding the felt with a base cloth, and then subjecting the felt to an impregnation treatment and curing and forming process to obtain a high-temperature resistant filter felt;

[0008] The glass fiber filter felt prepared by the above method has good air permeability, but its breaking strength is still low and its corrosion resistance is poor. Its breaking strength is significantly reduced in a high-temperature corrosion environment, which affects its performance. Summary of the invention

[0009] In order to solve the technical problems existing in the prior art, the present invention provides a glass fiber needle felt and a preparation method thereof, which improves the air permeability while ensuring the strength performance and still has high strength performance in a high temperature corrosive environment.

[0010] In view of the above technical problems, the present invention adopts the following technical solutions:

[0011] A method for preparing glass fiber needle felt is as follows:

[0012] 1. Glass fiber pretreatment

[0013] The glass fiber is placed in a hydrochloric acid solution, heated to 91-95°C at a rate of 1.2-1.4°C / min, and soaked at 91-95°C for 47-53min. After the soaking, the solution is filtered and dried to obtain acid-soaked glass fiber; the acid-soaked glass fiber is placed in an ethanol solution, and then sodium n-octadecyl sulfate and polyethylene glycol 200 are added. After stirring evenly, γ-aminopropyltriethoxysilane is added, and the solution is heated to 71-75°C at a rate of 1.8-2.2°C / min, and the solution is kept warm for reaction for 3.3-3.7h. After the reaction is completed, the solution is filtered, washed, and dried to obtain pretreated glass fiber;

[0014] The glass fiber has a diameter of 4.5-5.5 μm and a length of 47-53 mm;

[0015] The mass concentration of the hydrochloric acid solution is 14-16%;

[0016] The mass ratio of the glass fiber to the hydrochloric acid solution is 13-17:115-125;

[0017] The mass concentration of the ethanol solution is 60-64%;

[0018] The mass ratio of the acid-impregnated glass fiber, ethanol solution, sodium n-octadecyl sulfate, polyethylene glycol 200, and γ-aminopropyltriethoxysilane is 11.0-11.4:106-114:0.8-1.0:0.5-0.7:1.0-1.2.

[0019] 2. Preparation of primary glass fiber needle felt

[0020] The pretreated glass fiber is cut into short filaments with a length of 28-32 mm, and then respectively loosened and mixed, and then fed into a carding machine for a carding process to be processed into two groups of single fiber webs, and then cross-laid by a web laying machine, and a layer of plain weave polytetrafluoroethylene-based cloth is added to form a fiber web-base cloth-fiber web structure, and then needle-punched and reinforced by a pre-puncture-main puncture 1-main puncture 2 process to obtain a primary glass fiber needle-punched felt;

[0021] The polytetrafluoroethylene cloth has a gram weight of 78-82 g / m 2 ;

[0022] The web forming speed of the carding machine is 61-65m / min;

[0023] The reciprocating speed of the web laying machine is 61-65 m / min, and the forward moving speed is 5.0-6.0 m / min;

[0024] The pre-puncture depth is 9.3-9.7 mm, and the puncture density is 38-42 p / cm 2 The main puncture depth is 6.8-7.2mm, and the puncture density is 316-324p / cm 2 The main thorn 2 has a puncture depth of 6.0-6.4 mm and a puncture density of 355-365 p / cm 2 ;

[0025] The thickness of the primary glass fiber needle felt is 5.2-5.7 mm, and the density is 628-640 g / m 2 .

[0026] 3. Organize

[0027] (1) Preparation of silica particles

[0028] The tetraethyl orthosilicate, anhydrous ethanol and deionized water are mixed and stirred to obtain a mixed solution 1, 0.8-1.2 mol / L hydrochloric acid is added to the mixed solution 1 to adjust the pH to 3.4-3.6, and the mixture is stirred for 28-32 minutes at a stirring speed of 467-492 rpm. After the stirring is completed, 0.04-0.06 mol / L ammonia water is added to adjust the pH to 7.2-7.4, and the mixture is stirred for 15-19 minutes at a stirring speed of 512-526 rpm. After the stirring is completed, a mixed solution 2 is obtained, and cocamidopropyl hydroxysulfobetaine and glycerol are added to the mixed solution 2 for homogenization treatment, the homogenization time is 4.5-5.5 minutes, the homogenization pressure is 3.4-3.6 MPa, and after the homogenization treatment is completed, the mixture is placed in ethanol and allowed to stand for 46-50 hours at a standing temperature of 58-62° C., and the mixture is dried and ground to obtain silica particles;

[0029] The mass ratio of the tetraethyl orthosilicate, anhydrous ethanol and deionized water is 1.1-1.3:3.1-3.5:6.3-6.7;

[0030] The mass ratio of the mixed solution 2, cocamidopropyl hydroxysulfobetaine, glycerol and ethanol is 45-49:1.0-1.2:1.2-1.6:126-134;

[0031] (2) Preparation of modified silica particles

[0032] The silica gas particles are placed in an acetonitrile solution, stirred evenly, and then salicylic acid is added for ultrasonic treatment. The ultrasonic time is 21-25 minutes, the ultrasonic power is 67-71W, and the ultrasonic frequency is 20-24kHz. After the ultrasonic treatment, the temperature is raised to 71-75°C at a rate of 0.8-1.2°C / min, and a reflux reaction is performed. The reaction time is 21-23 hours. After the reaction is completed, the solution is filtered, washed, and dried to obtain modified silica particles.

[0033] The mass concentration of the acetonitrile solution is 21-25%;

[0034] The mass ratio of the silica particles, the acetonitrile solution and the salicylic acid is 11-13:495-504:22-24.

[0035] (3) Impregnation

[0036] The primary glass fiber needle felt is placed in an ethanol solution, modified silica particles, oleic acid amide and dodecyl hydroxyethyl dimethyl ammonium chloride are added, the temperature is raised to 61-66° C. at a rate of 1.8-2.2° C. / min, and the solution is allowed to stand for 35-40 minutes. After the solution is allowed to stand, the solution is dried to obtain the glass fiber needle felt;

[0037] The mass concentration of the ethanol solution is 40-44%;

[0038] The mass ratio of the primary glass fiber needle felt, the ethanol solution, the modified silicon dioxide particles, the oleic acid amide and the dodecyl hydroxyethyl dimethyl ammonium chloride is 18-22:140-150:13-17:1.6-1.8:1.6-2.0.

[0039] A glass fiber needle felt is prepared by the above-mentioned preparation method.

[0040] Compared with the prior art, the present invention has achieved the following beneficial effects:

[0041] 1. The present invention pre-treats the glass fiber, and uses sodium n-octadecyl sulfate as a surfactant, which, combined with polyethylene glycol 200, can fully penetrate into the interior of the glass fiber, improve the wetting performance of the glass fiber, improve the dispersion performance of the glass fiber, avoid the phenomenon of aggregation, and promote the entanglement performance of the fiber during needle punching. In addition, after aminosilane treatment, the friction coefficient of the glass fiber surface is improved, and the needle punching entanglement points of the glass fiber after needle punching are closely engaged, thereby enhancing the strength of the glass fiber, and the entanglement points do not slip or loosen in a high-temperature corrosive environment;

[0042] In the step of preparing silicon dioxide particles, cocamidopropyl hydroxysulfobetaine and glycerol are added to improve the dispersibility of silicon dioxide particles and increase the hydroxyl groups on the surface of silicon dioxide particles. Then, the silicon dioxide particles are reacted with salicylic acid. The carboxyl groups of salicylic acid and the hydroxyl groups of silicon dioxide particles are bonded to perform an esterification reaction. The primary glass fiber needle felt is impregnated with oleamide and dodecyl hydroxyethyl dimethyl ammonium chloride. First, the amino groups on the surface of the primary glass fiber needle felt can be bonded with the hydroxyl groups on the surface of the silicon dioxide particles, thereby enhancing the bonding force between the silicon dioxide particles and the primary glass fiber needle felt. The two are firmly connected, thereby giving full play to the effect of silicon dioxide. The particles enhance the performance of primary glass fiber needle felt, further improving the strength and high temperature corrosion resistance of the product. The silica particles have more pores and better permeability, which improves the air permeability of the product while ensuring the strength. Second, the esterification reaction cross-links salicylic acid and silica particles, and finally forms a cross-linked network structure of salicylic acid, silica particles and glass fiber needle felt, which has excellent stability. Third, oleic acid amide and dodecyl hydroxyethyl dimethyl ammonium chloride work synergistically, have good lubricity and softness, and thus promote the impregnation performance of primary glass fiber needle felt, enhancing the comprehensive performance of the product.

[0043] The present invention adopts a specific method to pretreat the glass fiber, combined with modified silica particles and impregnation and other technical means, to ensure the reinforcing performance of the silica particles for the primary glass fiber needle felt, and the two are closely combined with stable performance, while improving the air permeability, ensuring the strong performance and high temperature corrosion resistance, and achieving unexpected technical effects;

[0044] 2. The glass fiber needle felt prepared by the present invention has an air permeability of 1122-1150 m 3 / (m 2 h) -1 ;

[0045] 3. The glass fiber needle felt prepared by the present invention has a breaking strength of 1832-1857N and a tensile strength of 100.8-103.4N;

[0046] 4. The glass fiber needle felt prepared by the present invention was placed in a sealed container, and 3 times the mass of 20wt% hydrochloric acid solution was introduced, the temperature was controlled to 130°C, and it was allowed to stand for 72 hours. After standing, it was washed and dried, and the strength performance was tested again. The breaking strength was measured to be 1753-1798N, and the tensile strength was 96.8-100.4N;

[0047] Place it in a sealed container, pass 3 times the mass of 25wt% sodium hydroxide solution, control the temperature to 130℃, let it stand for 72h, wash and dry it after standing, and test the strength performance again. The breaking strength is measured to be 1737-1777N and the tensile strength is 95.9-99.5N. DETAILED DESCRIPTION

[0048] In order to more clearly understand the technical features, purposes and effects of the present invention, specific embodiments of the present invention are now described.

[0049] Example 1

[0050] 1. Glass fiber pretreatment

[0051] 15g of glass fiber is placed in 120g of hydrochloric acid solution, and the temperature is increased to 93°C at a rate of 1.3°C / min, and the solution is soaked at 93°C for 50min. After the soaking, the solution is filtered and dried to obtain acid-soaked glass fiber; 11.2g of the acid-soaked glass fiber is placed in 110g of ethanol solution, and then 0.9g of sodium n-octadecyl sulfate and 0.6g of polyethylene glycol 200 are added, and after stirring evenly, 1.1g of γ-aminopropyltriethoxysilane is added, and the temperature is increased to 73°C at a rate of 2.0°C / min, and the solution is kept warm for reaction for 3.5h. After the reaction is completed, the solution is filtered, washed, and dried to obtain pretreated glass fiber;

[0052] The glass fiber has a diameter of 5 μm and a length of 50 mm;

[0053] The mass concentration of the hydrochloric acid solution is 15%;

[0054] The mass concentration of the ethanol solution is 62%.

[0055] 2. Preparation of primary glass fiber needle felt

[0056] The pretreated glass fiber is cut into short filaments with a length of 30 mm, and then respectively loosened and mixed, and then fed into a carding machine for a carding process to be processed into two groups of single fiber webs, and then cross-laid by a web laying machine, and a layer of plain weave polytetrafluoroethylene-based cloth is added to form a fiber web-base cloth-fiber web structure, and then needle-punched and reinforced by a pre-puncture-main puncture 1-main puncture 2 process to obtain a primary glass fiber needle-punched felt;

[0057] The polytetrafluoroethylene cloth has a gram weight of 80 g / m 2 ;

[0058] The web forming speed of the carding machine is 63m / min;

[0059] The reciprocating speed of the web laying machine is 63m / min, and the forward moving speed is 5.5m / min;

[0060] The pre-puncture depth is 9.5 mm and the puncture density is 40 p / cm 2 The main puncture depth is 7.0 mm, and the puncture density is 320 p / cm 2 The main puncture depth of 2 is 6.2 mm, and the puncture density is 360 p / cm 2 ;

[0061] The thickness of the primary glass fiber needle felt is 5.5 mm and the density is 634 g / m 2 .

[0062] 3. Organize

[0063] (1) Preparation of silica particles

[0064] TEOS, anhydrous ethanol and deionized water were mixed and stirred to obtain a mixed solution 1, 1 mol / L hydrochloric acid was added to the mixed solution 1 to adjust the pH to 3.5, and the mixture was stirred for 30 min at a stirring speed of 480 rpm. After the stirring, 0.05 mol / L ammonia water was added to adjust the pH to 7.3, and the mixture was stirred for 17 min at a stirring speed of 520 rpm. After the stirring, a mixed solution 2 was obtained, and cocamidopropyl hydroxysulfobetaine and glycerol were added to the mixed solution 2 for homogenization treatment, the homogenization time was 5.0 min, the homogenization pressure was 3.5 MPa, and after the homogenization treatment, the mixture was placed in ethanol and allowed to stand for 48 h at a standing temperature of 60° C., and dried and ground to obtain silica particles;

[0065] The mass ratio of tetraethyl orthosilicate, anhydrous ethanol and deionized water is 1.2:3.3:6.5;

[0066] The mass ratio of the mixed solution 2, cocamidopropyl hydroxysulfobetaine, glycerol and ethanol is 47: 1.1: 1.4: 130;

[0067] (2) Preparation of modified silica particles

[0068] 12 g of silica particles were placed in 500 g of acetonitrile solution, and after stirring evenly, 23 g of salicylic acid was added for ultrasonic treatment. The ultrasonic time was 23 min, the ultrasonic power was 69 W, and the ultrasonic frequency was 22 kHz. After the ultrasonic treatment, the temperature was raised to 73 ° C at a rate of 1.0 ° C / min, and a reflux reaction was carried out. The reaction time was 22 h. After the reaction was completed, the solution was filtered, washed, and dried to obtain modified silica particles;

[0069] The mass concentration of the acetonitrile solution is 23%;

[0070] (3) Impregnation

[0071] 20 g of primary glass fiber needle felt was placed in 145 g of ethanol solution, 15 g of modified silica particles, 1.7 g of oleic acid amide and 1.8 g of dodecyl hydroxyethyl dimethyl ammonium chloride were added, the temperature was raised to 63° C. at a rate of 2.0° C. / min, and the solution was allowed to stand for 37 min. After the solution was allowed to stand, the solution was dried to obtain a glass fiber needle felt;

[0072] The mass concentration of the ethanol solution is 42%.

[0073] Example 2

[0074] 1. Glass fiber pretreatment

[0075] 13 g of glass fiber was placed in 115 g of hydrochloric acid solution, and the temperature was increased to 91° C. at a rate of 1.2° C. / min, and the solution was soaked at 91° C. for 47 min. After the soaking, the solution was filtered and dried to obtain acid-soaked glass fiber; 11.0 g of the acid-soaked glass fiber was placed in 106 g of ethanol solution, and then 0.8 g of sodium n-octadecyl sulfate and 0.5 g of polyethylene glycol 200 were added, and 1.0 g of γ-aminopropyltriethoxysilane was added after stirring evenly, and the temperature was increased to 71° C. at a rate of 1.8° C. / min, and the solution was kept warm for reaction for 3.3 h. After the reaction was completed, the solution was filtered, washed, and dried to obtain pretreated glass fiber;

[0076] The glass fiber has a diameter of 4.5 μm and a length of 47 mm;

[0077] The mass concentration of the hydrochloric acid solution is 14%;

[0078] The mass concentration of the ethanol solution is 60%.

[0079] 2. Preparation of primary glass fiber needle felt

[0080] The pretreated glass fiber is cut into short filaments with a length of 28 mm, and then respectively loosened and mixed, and then fed into a carding machine for a carding process to be processed into two groups of single fiber webs, and then cross-laid by a web laying machine, and a layer of plain weave polytetrafluoroethylene-based cloth is added to form a fiber web-base cloth-fiber web structure, and then needle-punched and reinforced by a pre-puncture-main puncture 1-main puncture 2 process to obtain a primary glass fiber needle-punched felt;

[0081] The polytetrafluoroethylene cloth has a gram weight of 78 g / m 2 ;

[0082] The web forming speed of the carding machine is 61m / min;

[0083] The reciprocating speed of the web laying machine is 61m / min, and the forward moving speed is 5.0m / min;

[0084] The pre-puncture depth is 9.3 mm and the puncture density is 38 p / cm2 The main puncture depth is 6.8 mm, and the puncture density is 316 p / cm 2 The main thorn 2 has a puncture depth of 6.0 mm and a puncture density of 355 p / cm 2 ;

[0085] The thickness of the primary glass fiber needle felt is 5.2 mm and the density is 628 g / m 2 .

[0086] 3. Organize

[0087] (1) Preparation of silica particles

[0088] TEOS, anhydrous ethanol and deionized water were mixed and stirred to obtain a mixed solution 1, 0.8 mol / L hydrochloric acid was added to the mixed solution 1 to adjust the pH to 3.4, and the mixture was stirred for 28 min at a stirring speed of 467 rpm. After the stirring, 0.04 mol / L ammonia water was added to adjust the pH to 7.2, and the mixture was stirred for 15 min at a stirring speed of 512 rpm. After the stirring, a mixed solution 2 was obtained, and cocamidopropyl hydroxysulfobetaine and glycerol were added to the mixed solution 2 for homogenization treatment, the homogenization time was 4.5 min, the homogenization pressure was 3.4 MPa, and after the homogenization treatment, the mixture was placed in ethanol and allowed to stand for 46 h at a standing temperature of 58° C., and dried and ground to obtain silica particles;

[0089] The mass ratio of the tetraethyl orthosilicate, anhydrous ethanol and deionized water is 1.1:3.1:6.3;

[0090] The mass ratio of the mixed solution 2, cocamidopropyl hydroxysulfobetaine, glycerol and ethanol is 45: 1.0: 1.2: 126;

[0091] (2) Preparation of modified silica particles

[0092] 11 g of silica particles were placed in 495 g of acetonitrile solution, and after stirring evenly, 22 g of salicylic acid was added for ultrasonic treatment. The ultrasonic time was 21 min, the ultrasonic power was 67 W, and the ultrasonic frequency was 20 kHz. After the ultrasonic treatment, the temperature was raised to 71 ° C at a rate of 0.8 ° C / min, and a reflux reaction was carried out. The reaction time was 21 h. After the reaction was completed, the solution was filtered, washed, and dried to obtain modified silica particles;

[0093] The mass concentration of the acetonitrile solution is 21%;

[0094] (3) Impregnation

[0095] 18 g of primary glass fiber needle felt was placed in 140 g of ethanol solution, 13 g of modified silica particles, 1.6 g of oleic acid amide and 1.6 g of dodecyl hydroxyethyl dimethyl ammonium chloride were added, the temperature was raised to 61° C. at a rate of 1.8° C. / min, and the solution was allowed to stand for 35 min. After the solution was allowed to stand, the solution was dried to obtain a glass fiber needle felt;

[0096] The mass concentration of the ethanol solution is 40%.

[0097] Example 3

[0098] 1. Glass fiber pretreatment

[0099] 17g of glass fiber is placed in 125g of hydrochloric acid solution, and the temperature is increased to 95°C at a rate of 1.4°C / min, and the solution is soaked at 95°C for 53min. After the soaking, the solution is filtered and dried to obtain acid-soaked glass fiber; 11.4g of acid-soaked glass fiber is placed in 114g of ethanol solution, and then 1.0g of sodium n-octadecyl sulfate and 0.7g of polyethylene glycol 200 are added, and 1.2g of γ-aminopropyltriethoxysilane is added after stirring evenly, and the temperature is increased to 75°C at a rate of 2.2°C / min, and the solution is kept warm for reaction for 3.7h. After the reaction is completed, the solution is filtered, washed, and dried to obtain pretreated glass fiber;

[0100] The glass fiber has a diameter of 5.5 μm and a length of 53 mm;

[0101] The mass concentration of the hydrochloric acid solution is 16%;

[0102] The mass concentration of the ethanol solution is 64%.

[0103] 2. Preparation of primary glass fiber needle felt

[0104] The pretreated glass fiber is cut into short filaments with a length of 32 mm, and then respectively loosened and mixed, and then fed into a carding machine for a carding process to be processed into two groups of single fiber webs, and then cross-laid by a web laying machine, and a layer of plain weave polytetrafluoroethylene-based cloth is added to form a fiber web-base cloth-fiber web structure, and then needle-punched and reinforced by a pre-puncture-main puncture 1-main puncture 2 process to obtain a primary glass fiber needle-punched felt;

[0105] The polytetrafluoroethylene cloth has a gram weight of 82 g / m 2 ;

[0106] The web forming speed of the carding machine is 65m / min;

[0107] The reciprocating speed of the web laying machine is 65m / min, and the forward moving speed is 6.0m / min;

[0108] The pre-puncture depth is 9.7 mm and the puncture density is 42 p / cm2 The main puncture depth is 7.2 mm, and the puncture density is 324 p / cm 2 The main puncture depth of 2 is 6.4 mm, and the puncture density is 365 p / cm 2 ;

[0109] The thickness of the primary glass fiber needle felt is 5.7 mm and the density is 640 g / m 2 .

[0110] 3. Organize

[0111] (1) Preparation of silica particles

[0112] TEOS, anhydrous ethanol and deionized water were mixed and stirred to obtain a mixed solution 1, 1.2 mol / L hydrochloric acid was added to the mixed solution 1 to adjust the pH to 3.6, and the mixture was stirred for 32 min at a stirring speed of 492 rpm. After the stirring, 0.06 mol / L ammonia water was added to adjust the pH to 7.4, and the mixture was stirred for 19 min at a stirring speed of 526 rpm. After the stirring, a mixed solution 2 was obtained, and cocamidopropyl hydroxysulfobetaine and glycerol were added to the mixed solution 2 for homogenization treatment, the homogenization time was 5.5 min, the homogenization pressure was 3.6 MPa, and after the homogenization treatment, the mixture was placed in ethanol and allowed to stand for 50 h at a standing temperature of 62° C., and dried and ground to obtain silica particles;

[0113] The mass ratio of tetraethyl orthosilicate, anhydrous ethanol and deionized water is 1.3:3.5:6.7;

[0114] The mass ratio of the mixed solution 2, cocamidopropyl hydroxysulfobetaine, glycerol and ethanol is 49: 1.2: 1.6: 134;

[0115] (2) Preparation of modified silica particles

[0116] 13 g of silica particles were placed in 504 g of acetonitrile solution, and after stirring, 24 g of salicylic acid was added for ultrasonic treatment. The ultrasonic time was 25 min, the ultrasonic power was 71 W, and the ultrasonic frequency was 24 kHz. After the ultrasonic treatment, the temperature was raised to 75 ° C at a rate of 1.2 ° C / min, and a reflux reaction was carried out. The reaction time was 23 h. After the reaction was completed, the solution was filtered, washed, and dried to obtain modified silica particles;

[0117] The mass concentration of the acetonitrile solution is 25%;

[0118] (3) Impregnation

[0119] 22 g of primary glass fiber needle felt was placed in 150 g of ethanol solution, 17 g of modified silica particles, 1.8 g of oleic acid amide and 2.0 g of dodecyl hydroxyethyl dimethyl ammonium chloride were added, the temperature was raised to 66° C. at a rate of 2.2° C. / min, and the solution was allowed to stand for 40 min. After the solution was allowed to stand, the solution was dried to obtain a glass fiber needle felt;

[0120] The mass concentration of the ethanol solution is 44%.

[0121] Comparative Example 1

[0122] Based on Example 1, the changes are as follows:

[0123] (1) The pretreatment step of the glass fiber is to place 15g of the glass fiber in 120g of hydrochloric acid solution, heat it to 93°C at a rate of 1.3°C / min, soak it at 93°C for 50min, filter it after soaking, and dry it to obtain acid-soaked glass fiber; the diameter of the glass fiber is 5μm and the length is 50mm; the mass concentration of the hydrochloric acid solution is 15%;

[0124] In the step of preparing the primary glass fiber needle felt, the pretreated glass fibers are replaced by acid-impregnated glass fibers in equal amounts;

[0125] (2) in the impregnation step, oleic acid amide and dodecyl hydroxyethyl dimethyl ammonium chloride components are omitted and oleic acid amide and dodecyl hydroxyethyl dimethyl ammonium chloride are replaced with equal amounts of oleic acid amide and dodecyl hydroxyethyl dimethyl ammonium chloride in the impregnation solution;

[0126] The rest of the operations are the same.

[0127] Comparative Example 2

[0128] Based on Example 1, the changes are as follows:

[0129] (1) In the step of preparing silica particles, the operation step of “adding cocamidopropyl hydroxysulfobetaine and glycerol to the mixed solution 2 for homogenization, the homogenization time is 5.0 min, the homogenization pressure is 3.5 MPa, and after the homogenization is completed” is omitted;

[0130] That is, the mixed solution 2 is placed in ethanol and allowed to stand for 48 hours at a temperature of 60° C., and then dried and ground to obtain silicon dioxide particles;

[0131] The mass ratio of the second mixed solution to ethanol is 47:130;

[0132] (2) The step of preparing modified silica particles is omitted, and in the impregnation step, an equal amount of modified silica particles is replaced by silica particles;

[0133] The rest of the operations are the same.

[0134] Test example

[0135] 1. Breathability

[0136] The air permeability test of the glass fiber needle felts prepared in Examples 1-3 and Comparative Examples 1-2 was performed, and the results were as follows:

[0137]

[0138] 2. Strong performance

[0139] The glass fiber needle felts prepared in Examples 1-3 and Comparative Examples 1-2 were tested for strength performance, and the results were as follows:

[0140]

[0141] 3. High temperature corrosion resistance

[0142] (1) Acid corrosion

[0143] The glass fiber needle felt prepared in Example 1-3 and Comparative Example 1-2 was placed in a sealed container, and 3 times the mass of 20wt% hydrochloric acid solution was introduced. The temperature was controlled at 130°C, and the felt was allowed to stand for 72 hours. After standing, it was washed and dried, and the strength performance was tested again. The results are as follows:

[0144]

[0145] (2) Alkali corrosion

[0146] The glass fiber needle felt prepared in Example 1-3 and Comparative Example 1-2 was placed in a sealed container, and 3 times the mass of 25wt% sodium hydroxide solution was introduced. The temperature was controlled at 130°C, and the felt was allowed to stand for 72 hours. After standing, it was washed and dried, and the strength performance was tested again. The results are as follows:

[0147]

[0148] The present invention pre-treats the glass fiber, and uses n-octadecyl sulfate as a surfactant, which, combined with polyethylene glycol 200, can fully penetrate into the interior of the glass fiber, improve the wetting performance of the glass fiber, improve the dispersion performance of the glass fiber, avoid the phenomenon of aggregation, and promote the entanglement performance of the fiber during needle punching. In addition, after aminosilane treatment, the friction coefficient of the glass fiber surface is improved, and the needle punching entanglement points of the glass fiber after needle punching are closely engaged, thereby enhancing the strength performance of the glass fiber, and the slippage and loosening of the entanglement points do not occur in a high-temperature corrosive environment.

[0149] In the step of preparing silicon dioxide particles, cocamidopropyl hydroxysulfobetaine and glycerol are added to improve the dispersibility of silicon dioxide particles and increase the hydroxyl groups on the surface of silicon dioxide particles. Then, the silicon dioxide particles are reacted with salicylic acid. The carboxyl groups of salicylic acid and the hydroxyl groups of silicon dioxide particles are bonded to perform an esterification reaction. The primary glass fiber needle felt is impregnated with oleamide and dodecyl hydroxyethyl dimethyl ammonium chloride. First, the amino groups on the surface of the primary glass fiber needle felt can be bonded with the hydroxyl groups on the surface of the silicon dioxide particles, thereby enhancing the bonding force between the silicon dioxide particles and the primary glass fiber needle felt. The two are firmly connected, thereby giving full play to the effect of silicon dioxide. The particles enhance the performance of primary glass fiber needle felt, further improving the strength and high temperature corrosion resistance of the product. The silica particles have more pores and better permeability, which improves the air permeability of the product while ensuring the strength. Second, the esterification reaction cross-links salicylic acid and silica particles, and finally forms a cross-linked network structure of salicylic acid, silica particles and glass fiber needle felt, which has excellent stability. Third, oleic acid amide and dodecyl hydroxyethyl dimethyl ammonium chloride work synergistically, have good lubricity and softness, and thus promote the impregnation performance of primary glass fiber needle felt, enhancing the comprehensive performance of the product.

[0150] The present invention adopts a specific method to pretreat the glass fiber, combines modified silica particles and impregnation and other technical means, to ensure the reinforcing performance of the silica particles for the primary glass fiber needle felt, and the two are closely combined with stable performance, while improving the air permeability, ensuring the strength performance and high temperature corrosion resistance performance, and achieving unexpected technical effects.

[0151] In the glass fiber pretreatment step of Comparative Example 1, only the glass fiber is pretreated, and the obtained pretreated glass fiber has poor wetting performance, poor dispersion performance, and has a relatively serious aggregation phenomenon, which leads to poor entanglement performance of the fiber during needle punching, and the needle punching entanglement points are not tightly engaged, thereby reducing the strength performance of the product, and the entanglement points are prone to slippage and looseness in a high-temperature corrosion environment, which reduces the high-temperature corrosion resistance. In addition, oleic acid amide and dodecylhydroxyethyldimethylammonium chloride components are omitted in the impregnation step, resulting in insufficient impregnation, thereby reducing the impregnation performance of the primary glass fiber needle felt, and ultimately affecting the comprehensive performance of the product.

[0152] The silica particles prepared in Comparative Example 2 have poor dispersion performance. Although the prepared silica particles have hydroxyl groups that can be bonded with the amino groups of the primary glass fiber needle felt, the silica particles are in a clustered state and have poor permeability, which reduces the air permeability of the product. In addition, the bonding with the primary glass fiber needle felt is incomplete, resulting in a loose and weak connection between the silica particles and the primary glass fiber needle felt. In addition, Comparative Example 2 omits the modification step of the silica particles, and it is impossible to undergo esterification reaction and obtain a cross-linked network structure, which ultimately leads to poor reinforcement performance of the silica particles, poor strength performance of the product, and poor high-temperature corrosion resistance.

[0153] Unless otherwise specified, all ratios and percentages described in the present invention are by mass ratios and percentages are by mass percentages.

[0154] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a glass fiber needle felt, characterized in that: The preparation method comprises the steps of pre-treating glass fibers, preparing primary glass fiber needle felt, and finishing; The glass fiber pretreatment step comprises placing the acid-soaked glass fiber in an ethanol solution, then adding sodium octadecyl sulfate and polyethylene glycol 200, stirring evenly, adding γ-aminopropyltriethoxysilane, heating to 71-75° C. at a rate of 1.8-2.2° C. / min, keeping the temperature for reaction for 3.3-3.7 hours, filtering, washing and drying after the reaction is completed, to obtain the pretreated glass fiber; The finishing step includes preparing silica particles, preparing modified silica particles, and impregnation steps; The step of preparing the silicon dioxide particles is to mix ethyl orthosilicate, anhydrous ethanol and deionized water, stir evenly to obtain a mixed solution 1, add hydrochloric acid to the mixed solution 1 to adjust the pH to 3.4-3.6, stir once, add ammonia water to adjust the pH to 7.2-7.4 after the first stirring, stir twice, obtain a mixed solution 2 after the second stirring, add cocamidopropyl hydroxysulfobetaine and glycerol to the mixed solution 2 for homogenization, the homogenization time is 4.5-5.5min, the homogenization pressure is 3.4-3.6MPa, after the homogenization, place in ethanol and stand for 46-50h, the standing temperature is 58-62°C, dry and grind to obtain the silicon dioxide particles; The step of preparing the modified silicon dioxide particles is as follows: placing the silicon dioxide particles in an acetonitrile solution, stirring evenly, adding salicylic acid for ultrasonic treatment, and after the ultrasonic treatment, heating to 71-75° C. at a rate of 0.8-1.2° C. / min, performing a reflux reaction for 21-23 hours, and filtering, washing, and drying after the reaction to obtain the modified silicon dioxide particles; The impregnation step is to place the primary glass fiber needle felt in an ethanol solution, add modified silicon dioxide particles, oleic acid amide and dodecyl hydroxyethyl dimethyl ammonium chloride, heat to 61-66° C. at a rate of 1.8-2.2° C. / min, stand for 35-40 minutes, and dry after standing to obtain the glass fiber needle felt.

2. The method for preparing a glass fiber needle felt according to claim 1, characterized in that: In the step of pretreating the glass fiber, the method for preparing the acid-impregnated glass fiber is to place the glass fiber in a hydrochloric acid solution, heat it to 91-95°C at a rate of 1.2-1.4°C / min, soak it at 91-95°C for 47-53min, filter it after soaking, and dry it to obtain the acid-impregnated glass fiber; The glass fiber has a diameter of 4.5-5.5 μm and a length of 47-53 mm; The mass concentration of the hydrochloric acid solution is 14-16%; The mass ratio of the glass fiber to the hydrochloric acid solution is 13-17:115-125.

3. The method for preparing a glass fiber needle felt according to claim 1, characterized in that: In the step of pretreating the glass fiber, the mass concentration of the ethanol solution is 60-64%; The mass ratio of the acid-impregnated glass fiber, ethanol solution, sodium n-octadecyl sulfate, polyethylene glycol 200, and γ-aminopropyltriethoxysilane is 11.0-11.4:106-114:0.8-1.0:0.5-0.7:1.0-1.

2.

4. The method for preparing a glass fiber needle felt according to claim 1, characterized in that: The step of preparing the primary glass fiber needle felt is to cut the pretreated glass fiber into short filaments with a length of 28-32 mm, and then respectively open and mix them, feed them into a carding machine for a carding process, process them into two groups of single fiber webs, and then cross-lay them through a web laying machine, and add a layer of polytetrafluoroethylene cloth with a plain weave structure to form a fiber web-base cloth-fiber web structure, and then perform needle punching reinforcement through a pre-puncture-main puncture 1-main puncture 2 process to obtain the primary glass fiber needle felt; The polytetrafluoroethylene cloth has a gram weight of 78-82 g / m 2 ; The web forming speed of the carding machine is 61-65m / min; The reciprocating speed of the web laying machine is 61-65 m / min, and the forward moving speed is 5.0-6.0 m / min; The pre-puncture depth is 9.3-9.7 mm, and the puncture density is 38-42 p / cm 2 The main puncture depth is 6.8-7.2mm, and the puncture density is 316-324p / cm 2 The main thorn 2 has a puncture depth of 6.0-6.4 mm and a puncture density of 355-365 p / cm 2 ; The thickness of the primary glass fiber needle felt is 5.2-5.7 mm, and the density is 628-640 g / m 2 .

5. The method for preparing a glass fiber needle felt according to claim 1, characterized in that: In the step of preparing the silicon dioxide particles, the stirring time of the stirring is 28-32 minutes, and the stirring speed is 467-492 rpm; The stirring time of the secondary stirring is 15-19 min, and the stirring speed is 512-526 rpm.

6. The method for preparing a glass fiber needle felt according to claim 1, characterized in that: In the step of preparing the silicon dioxide particles, the concentration of the hydrochloric acid is 0.8-1.2 mol / L; The concentration of the ammonia water is 0.04-0.06 mol / L; The mass ratio of the tetraethyl orthosilicate, anhydrous ethanol and deionized water is 1.1-1.3:3.1-3.5:6.3-6.7; The mass ratio of the mixed solution 2, cocamidopropyl hydroxysulfobetaine, glycerol and ethanol is 45-49: 1.0-1.2: 1.2-1.6: 126-134.

7. The method for preparing a glass fiber needle felt according to claim 1, characterized in that: In the step of preparing the modified silicon dioxide particles, the ultrasonic treatment has an ultrasonic time of 21-25 min, an ultrasonic power of 67-71 W, and an ultrasonic frequency of 20-24 kHz; The mass concentration of the acetonitrile solution is 21-25%; The mass ratio of the silica particles, the acetonitrile solution and the salicylic acid is 11-13:495-504:22-24.

8. The method for preparing a glass fiber needle felt according to claim 1, characterized in that: In the step of impregnating, the mass concentration of the ethanol solution is 40-44%; The mass ratio of the primary glass fiber needle felt, the ethanol solution, the modified silicon dioxide particles, the oleic acid amide and the dodecyl hydroxyethyl dimethyl ammonium chloride is 18-22:140-150:13-17:1.6-1.8:1.6-2.

0.

9. Glass fiber needle felt obtained according to the preparation method according to any one of claims 1 to 8.