A method for preparing highly dispersed silicon dioxide
By using composite agent and crosslinking agent in the preparation process of silica, the problem of insufficient wear resistance and tensile properties of silica in the prior art is solved, and high dispersion is achieved The preparation of silica has good dispersion properties and stability.
Patent Information
- Application Number
- CN202411095521.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-12
AI Technical Summary
The highly dispersed silica prepared by the prior art improves the specific surface area and dispersion properties, and the wear resistance and tensile properties are insufficient, which affects its application effect in rubber matrix.
A specific method is used to prepare a mixed solution. The compound agent is used as a surfactant to enhance the dispersion of the sodium silicate solution, and the pH value is adjusted through stages and the addition of glyceryl monostearate, polyethylene glycol, and vinyl triethylene Oxysilane, thioglycolic acid and ethylenediamine form a stable crosslinking structure, and combined with high-temperature heat treatment, enhance the dispersion properties of silica and the wear resistance of vulcanized glue.
The obtained silica has a large specific surface area, good dispersion properties, enhanced wear resistance and tensile properties. The stable crosslinking structure avoids particle agglomeration and improves the strength and stability of the vulcanized rubber.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of silicon dioxide, and particularly relates to a method for preparing highly dispersed silicon dioxide. Background Art
[0002] Silica is a good reinforcing material for synthetic rubber. It can reduce tire rolling resistance and improve tire anti-skid ability. It can also be used in medicine, pesticide, coating, toothpaste, paper and cosmetics industries, and has a wide range of applications.
[0003] However, the silica prepared by existing enterprises usually increases the specific surface area while reducing the dispersion performance, affecting the dispersion in the rubber matrix and failing to give full play to its reinforcing performance;
[0004] In order to solve the above technical problems, the prior art discloses the following:
[0005] CN114368760A discloses a method for dispersing highly dispersed silicon dioxide, specifically disclosing the steps of mixing a turbid and sodium silicate aqueous solution with an alcohol-water mixture to obtain a primary mixed solution; mixing a mixed modified organic solution with the primary mixed solution to obtain a mixed solution; mixing the mixed solution with sulfuric acid, aging, to obtain a primary precipitate; mixing a mixed initiator with the primary precipitate, drying, and heat-treating the mixture to obtain highly dispersed silicon dioxide;
[0006] Although the highly dispersed silica produced by this patent has a higher specific surface area and better dispersion performance, its specific surface area is still relatively small.
[0007] CN117735562A discloses a highly reinforced and highly dispersed silicon dioxide and a preparation method thereof. Specifically, the preparation method is as follows: mixing a water glass solution and sulfuric acid to obtain a first reaction liquid, dripping sulfuric acid into the first reaction liquid at a first dripping speed, and simultaneously dripping a water glass solution to obtain a second reaction liquid, dripping sulfuric acid into the second reaction liquid at a second dripping speed, and simultaneously dripping a water glass solution to obtain a fourth reaction liquid, adjusting the pH to obtain a precipitated silicon dioxide suspension, and drying to obtain silicon dioxide;
[0008] The silicon dioxide produced by this patent has a large specific surface area and good dispersion performance, but the vulcanized rubber produced has poor wear resistance and poor tensile properties. Summary of the invention
[0009] In order to solve the technical problems existing in the prior art, the present invention provides a method for preparing highly dispersed silicon dioxide, which has a large specific surface area and good dispersion performance. The prepared vulcanized rubber can effectively enhance the wear resistance, good tensile performance and excellent stability.
[0010] In view of the above technical problems, the present invention adopts the following technical solutions:
[0011] A method for preparing highly dispersed silicon dioxide comprises the steps of preparing a mixed solution 1, preparing a mixed solution 2, preparing a mixed solution 3, preparing primary silicon dioxide, and heat treatment. The specific operations are as follows:
[0012] 1. Preparation of mixed solution
[0013] The sodium silicate solution and the composite agent are mixed, and then the temperature is raised to 60-64°C at a rate of 0.8-1.2°C / min for ultrasonic treatment, the ultrasonic time is 9-12min, the ultrasonic frequency is 25-30kHz, the ultrasonic power is 82-88W, and sulfuric acid solution is added after the ultrasonic treatment, the pH value is controlled to be 4.8-5.2, and the stirring is performed for 12-17min at a stirring speed of 104-115rpm. After the stirring is completed, a mixed solution 1 is obtained;
[0014] The mass concentration of the sodium silicate solution is 24-28%;
[0015] The compound is a mixture of sodium citrate, sodium sulfate of fatty alcohol polyoxyethylene ether and Tween 80, and the mass ratio of sodium citrate, sodium sulfate of fatty alcohol polyoxyethylene ether and Tween 80 is 1.8-2.2:3.2-3.6:2.4-2.6;
[0016] The mass ratio of the sodium silicate solution to the composite agent is 24-28:4.5-4.9;
[0017] The mass concentration of the sulfuric acid solution is 10.2-10.4%.
[0018] 2. Preparation of Mixture II
[0019] Add sodium silicate solution to mixed solution 1, stir evenly, control the addition rate to 1.0-1.4 mL / min, the system pH value is 8.7-8.9, continue to add sodium silicate solution, stir evenly, control the addition rate to 0.7-0.9 mL / min, the system pH value is 11.1-11.5, to obtain mixed solution 2;
[0020] The mass concentration of the sodium silicate solution is 24-28%.
[0021] 3. Preparation of Mixture III
[0022] Add sulfuric acid solution to the mixed solution 2, stir evenly, control the addition rate to 1.2-1.4 mL / min, the system pH value is 9.6-9.8, continue to add sulfuric acid solution, stir evenly, control the addition rate to 1.0-1.2 mL / min, the system pH value is 8.3-8.7, add sulfuric acid solution again, stir evenly, control the addition rate to 0.7-0.9 mL / min, the system pH value is 7.0, to obtain a mixed solution 3;
[0023] The mass concentration of the sulfuric acid solution is 10.2-10.4%.
[0024] 4. Preparation of Primary Silica
[0025] The mixed solution is placed in a sealed container, and then anhydrous ethanol is added. After stirring, glyceryl monostearate and polyethylene glycol are added for ultrasonic treatment. The ultrasonic time is 18-22 minutes and the ultrasonic power is 116-124W. After the ultrasonic treatment, vinyl triethoxysilane is added, and the temperature is raised to 80-84°C at a rate of 0.8-1.2°C / min, and the reaction is carried out for 3.8-4.2 hours. After the reaction is completed, thioglycolic acid and ethylenediamine are added, and after stirring, the temperature is controlled at 34-36°C, and ultraviolet irradiation is carried out. The ultraviolet wavelength is 235-245nm, and the irradiation time is 1.8-2.2 hours. After the irradiation is completed, it is filtered and freeze-dried. The freezing temperature is -37 to -33°C and the freezing time is 28-31 hours. After the freezing is completed, it is naturally restored to room temperature to obtain primary silicon dioxide;
[0026] The mass ratio of the mixed solution 3, anhydrous ethanol, glyceryl monostearate, polyethylene glycol, vinyl triethoxysilane, thioglycolic acid and ethylenediamine is 18-22:30-34:1.4-1.6:1.1-1.5:1.5-1.7:0.8-1.0:1.1-1.4.
[0027] 5. Heat treatment
[0028] The primary silicon dioxide is placed in a closed environment for heat treatment, firstly the temperature is increased to 195-205°C at a rate of 4.8-5.2°C / min, and the temperature is kept at 195-205°C for 37-43min, then the temperature is increased to 354-363°C at a rate of 2.8-3.2°C / min, and the temperature is kept at 354-363°C for 1.8-2.2h. After the heat preservation treatment, the temperature is naturally lowered to room temperature to obtain highly dispersed silicon dioxide.
[0029] Compared with the prior art, the present invention has achieved the following beneficial effects:
[0030] 1. The present invention adopts a specific method to prepare a mixed solution 1, wherein the composite agent as a surfactant can enhance the dispersibility of the sodium silicate solution, making the mixed solution 1 more uniform and stable, and it can better contact with the sulfuric acid solution, so that the reaction is more sufficient, ensuring that the silicon dioxide has a more stable skeleton and a uniform structure, and then the dispersibility of the silicon dioxide is regulated by adjusting the pH in a staged manner. In the step of preparing primary silicon dioxide, the monostearate and polyethylene glycol components can improve the uniform dispersibility of the mixed solution 3, and then vinyl triethoxysilane is added to enhance the hydrophobicity of the silicon dioxide and reduce the degree of aggregation, and then thioglycolic acid and ethylenediamine are introduced, wherein the vinyl group can be bonded with the thiol group, and the amino group of ethylenediamine can form a hydrogen bond with the carboxyl group of thioglycolic acid, and a stable cross-linked structure is formed therebetween to coat the surface of the silicon dioxide, and combined with high-temperature heat treatment, on the one hand, the dispersibility of the silicon dioxide can be enhanced, and the agglomeration between the particles is avoided, and the thermal stability is good; on the other hand, the stable cross-linked structure enhances the strength and wear resistance of the vulcanized rubber, reduces the loss, and makes the stability of the vulcanized rubber good;
[0031] 2. The silica prepared by the method of the present invention has a BET specific surface area of 308-315 m 2 / g, heating loss at 120℃ is 1.8-2.3%, and oil absorption value is 258-267mL / 100g;
[0032] 3. The silica prepared by the method of the present invention is used to prepare vulcanized rubber according to the standard of HG / T 2404-2020, and the wear loss of the vulcanized rubber is measured to be 115-119 mm 3 , loss factor 60℃tanδ is 0.061-0.067, tensile strength is 28.3-29.1MPa, and elongation at break is 594-603%;
[0033] 4. The silica prepared by the method of the present invention is used to prepare vulcanized rubber according to the standard of HG / T 2404-2020, and is placed at a temperature of 88°C for 120 hours. After the standing period, the mixture is naturally restored to room temperature, and then placed in a 24wt% sodium hydroxide solution with a mass of 4 times and immersed for 72 hours. After the immersion period, the mixture is washed and dried, and the tensile strength is measured again to be 27.3-28.4MPa, and the elongation at break is 570-584%. DETAILED DESCRIPTION
[0034] In order to more clearly understand the technical features, purposes and effects of the present invention, specific embodiments of the present invention are now described.
[0035] Example 1
[0036] 1. Preparation of mixed solution
[0037] 26 g of sodium silicate solution and 4.7 g of the composite agent were mixed, and then the temperature was raised to 62° C. at a rate of 1.0° C. / min for ultrasonic treatment. The ultrasonic time was 10 min, the ultrasonic frequency was 27 kHz, and the ultrasonic power was 85 W. After the ultrasonic treatment, sulfuric acid solution was added, the pH value was controlled to be 5, and the mixture was stirred for 14 min at a stirring speed of 110 rpm. After the stirring was completed, a mixed solution 1 was obtained;
[0038] The mass concentration of the sodium silicate solution is 26%;
[0039] The compound is a mixture of sodium citrate, sodium sulfate of fatty alcohol polyoxyethylene ether and Tween 80, and the mass ratio of sodium citrate, sodium sulfate of fatty alcohol polyoxyethylene ether and Tween 80 is 2.0:3.4:2.5;
[0040] The mass concentration of the sulfuric acid solution is 10.3%.
[0041] 2. Preparation of Mixture II
[0042] Add sodium silicate solution to mixed solution 1, stir evenly, control the addition rate to 1.2 mL / min, the system pH value is 8.8, continue to add sodium silicate solution, stir evenly, control the addition rate to 0.8 mL / min, the system pH value is 11.3, to obtain mixed solution 2;
[0043] The mass concentration of the sodium silicate solution is 26%.
[0044] 3. Preparation of Mixture III
[0045] Add sulfuric acid solution to the mixed solution 2, stir evenly, control the addition rate to 1.3 mL / min, the system pH value is 9.7, continue to add sulfuric acid solution, stir evenly, control the addition rate to 1.1 mL / min, the system pH value is 8.5, add sulfuric acid solution again, stir evenly, control the addition rate to 0.8 mL / min, the system pH value is 7.0, to obtain a mixed solution 3;
[0046] The mass concentration of the sulfuric acid solution is 10.3%.
[0047] 4. Preparation of Primary Silica
[0048] Place 20g of the mixed solution in a sealed container, then add 32g of anhydrous ethanol, stir evenly, add 1.5g of glyceryl monostearate and 1.3g of polyethylene glycol, and carry out ultrasonic treatment. The ultrasonic time is 20min and the ultrasonic power is 120W. After the ultrasonic treatment, add 1.6g of vinyltriethoxysilane, heat to 82°C at a rate of 1.0°C / min, and react for 4.0h. After the reaction, add 0.9g of thioglycolic acid and 1.3g of ethylenediamine, stir evenly, control the temperature to 35°C, and carry out ultraviolet irradiation with an ultraviolet wavelength of 240nm and an irradiation time of 2.0h. After the irradiation, filter and freeze-dry. The freezing temperature is -35°C and the freezing time is 30h. After the freezing, naturally return to room temperature to obtain primary silica.
[0049] 5. Heat treatment
[0050] The primary silica was placed in a closed environment for heat treatment, firstly the temperature was increased to 200°C at a rate of 5.0°C / min, and kept at 200°C for 40 minutes, then the temperature was increased to 360°C at a rate of 3.0°C / min, and kept at 360°C for 2.0 hours. After the heat preservation treatment, the temperature was naturally lowered to room temperature to obtain highly dispersed silica.
[0051] Example 2
[0052] 1. Preparation of mixed solution
[0053] 24 g of sodium silicate solution and 4.5 g of the composite agent were mixed, and then the temperature was raised to 60° C. at a rate of 0.8° C. / min for ultrasonic treatment. The ultrasonic time was 9 min, the ultrasonic frequency was 25 kHz, and the ultrasonic power was 82 W. After the ultrasonic treatment, sulfuric acid solution was added, the pH value was controlled to be 4.8, and the mixture was stirred for 12 min at a stirring speed of 104 rpm. After the stirring was completed, a mixed solution 1 was obtained;
[0054] The mass concentration of the sodium silicate solution is 24%;
[0055] The compound is a mixture of sodium citrate, sodium sulfate of fatty alcohol polyoxyethylene ether and Tween 80, and the mass ratio of sodium citrate, sodium sulfate of fatty alcohol polyoxyethylene ether and Tween 80 is 1.8:3.2:2.4;
[0056] The mass concentration of the sulfuric acid solution is 10.2%.
[0057] 2. Preparation of Mixture II
[0058] Add sodium silicate solution to mixed solution 1, stir evenly, control the addition rate to 1.0 mL / min, the system pH value is 8.7, continue to add sodium silicate solution, stir evenly, control the addition rate to 0.7 mL / min, the system pH value is 11.1, to obtain mixed solution 2;
[0059] The mass concentration of the sodium silicate solution is 24%.
[0060] 3. Preparation of Mixture III
[0061] Add sulfuric acid solution to the mixed solution 2, stir evenly, control the addition rate to 1.2 mL / min, the system pH value is 9.6, continue to add sulfuric acid solution, stir evenly, control the addition rate to 1.0 mL / min, the system pH value is 8.3, add sulfuric acid solution again, stir evenly, control the addition rate to 0.7 mL / min, the system pH value is 7.0, to obtain a mixed solution 3;
[0062] The mass concentration of the sulfuric acid solution is 10.2%.
[0063] 4. Preparation of Primary Silica
[0064] Place 18g of the mixed solution in a sealed container, then add 30g of anhydrous ethanol, stir evenly, add 1.4g of glyceryl monostearate and 1.1g of polyethylene glycol, and carry out ultrasonic treatment. The ultrasonic time is 18min and the ultrasonic power is 116W. After the ultrasonic treatment, add 1.5g of vinyltriethoxysilane, heat to 80°C at a rate of 0.8°C / min, and react for 3.8h. After the reaction, add 0.8g of thioglycolic acid and 1.1g of ethylenediamine, stir evenly, control the temperature to 34°C, and carry out ultraviolet irradiation with an ultraviolet wavelength of 235nm and an irradiation time of 1.8h. After the irradiation, filter and freeze-dry. The freezing temperature is -37°C and the freezing time is 28h. After the freezing, it naturally returns to room temperature to obtain primary silica.
[0065] 5. Heat treatment
[0066] The primary silica was placed in a closed environment for heat treatment. The temperature was first increased to 195°C at a rate of 4.8°C / min, and kept at 195°C for 37 minutes. The temperature was then increased to 354°C at a rate of 2.8°C / min, and kept at 354°C for 1.8 hours. After the insulation treatment, the temperature was naturally lowered to room temperature to obtain highly dispersed silica.
[0067] Example 3
[0068] 1. Preparation of mixed solution
[0069] 28g of sodium silicate solution and 4.9g of the composite agent were mixed, and then the temperature was raised to 64°C at a rate of 1.2°C / min for ultrasonic treatment. The ultrasonic time was 12min, the ultrasonic frequency was 30kHz, and the ultrasonic power was 88W. After the ultrasonic treatment, sulfuric acid solution was added, the pH value was controlled to be 5.2, and the mixture was stirred for 17min at a stirring speed of 115rpm. After the stirring was completed, a mixed solution 1 was obtained;
[0070] The mass concentration of the sodium silicate solution is 28%;
[0071] The compound is a mixture of sodium citrate, sodium sulfate of fatty alcohol polyoxyethylene ether and Tween 80, and the mass ratio of sodium citrate, sodium sulfate of fatty alcohol polyoxyethylene ether and Tween 80 is 2.2:3.6:2.6;
[0072] The mass concentration of the sulfuric acid solution is 10.4%.
[0073] 2. Preparation of Mixture II
[0074] Add sodium silicate solution to mixed solution 1, stir evenly, control the addition rate to 1.4 mL / min, the system pH value is 8.9, continue to add sodium silicate solution, stir evenly, control the addition rate to 0.9 mL / min, the system pH value is 11.5, to obtain mixed solution 2;
[0075] The mass concentration of the sodium silicate solution is 28%.
[0076] 3. Preparation of Mixture III
[0077] Add sulfuric acid solution to the mixed solution 2, stir evenly, control the addition rate to 1.4 mL / min, the system pH value is 9.8, continue to add sulfuric acid solution, stir evenly, control the addition rate to 1.2 mL / min, the system pH value is 8.7, add sulfuric acid solution again, stir evenly, control the addition rate to 0.9 mL / min, the system pH value is 7.0, to obtain a mixed solution 3;
[0078] The mass concentration of the sulfuric acid solution is 10.4%.
[0079] 4. Preparation of Primary Silica
[0080] Place 22g of the mixed solution in a sealed container, then add 34g of anhydrous ethanol, stir evenly, add 1.6g of glyceryl monostearate and 1.5g of polyethylene glycol, and carry out ultrasonic treatment. The ultrasonic time is 22min and the ultrasonic power is 124W. After the ultrasonic treatment, add 1.7g of vinyltriethoxysilane, heat to 84°C at a rate of 1.2°C / min, and react for 4.2h. After the reaction, add 1.0g of thioglycolic acid and 1.4g of ethylenediamine, stir evenly, control the temperature to 36°C, and carry out ultraviolet irradiation with an ultraviolet wavelength of 245nm and an irradiation time of 2.2h. After the irradiation, filter and freeze-dry. The freezing temperature is -33°C and the freezing time is 31h. After the freezing, it naturally returns to room temperature to obtain primary silica.
[0081] 5. Heat treatment
[0082] The primary silica was placed in a closed environment for heat treatment. The temperature was first increased to 205°C at a rate of 5.2°C / min, and kept at 205°C for 43 minutes. The temperature was then increased to 363°C at a rate of 3.2°C / min, and kept at 363°C for 2.2 hours. After the insulation treatment, the temperature was naturally lowered to room temperature to obtain highly dispersed silica.
[0083] Comparative Example 1
[0084] Based on Example 1, the change is that the step of preparing primary silicon dioxide is to filter the mixed solution 3 and freeze-dry it, the freezing temperature is -35°C, the freezing time is 30 hours, and the freezing is completed to obtain primary silicon dioxide;
[0085] The rest of the operations are the same;
[0086] Comparative Example 2
[0087] Based on Example 1, the changes are as follows:
[0088] (1) In the step of preparing the mixed solution, the composite agent components were replaced with deionized water in equal amounts, and the rest of the operations were the same;
[0089] (2) The step of preparing the mixed solution 2 is to add the sodium silicate solution to the mixed solution 1, stir evenly, control the addition rate to be 1.2 mL / min, and the pH value of the system is 11.3, to obtain the mixed solution 2; the mass concentration of the sodium silicate solution is 26%;
[0090] (3) The step of preparing the mixed solution three is to add sulfuric acid solution to the mixed solution two, stir evenly, control the addition rate to be 1.3 mL / min, and the pH value of the system is 7.0, to obtain the mixed solution three; the mass concentration of the sulfuric acid solution is 10.3%;
[0091] The rest of the operations are the same.
[0092] Test example
[0093] (1) Performance of highly dispersed silica
[0094] The highly dispersed silica obtained in Example 1-3 and Comparative Example 1-2 was tested, and the results were as follows:
[0095]
[0096] (2) Vulcanized rubber made from highly dispersed silica
[0097] The highly dispersed silica obtained in Examples 1-3 and Comparative Examples 1-2 was used to prepare vulcanized rubber according to the standard of HG / T 2404-2020, and the wear resistance and strength properties were tested. The test frequency of the vulcanized rubber loss factor tanδ was 50 Hz, the dynamic strain was 1%, and the test temperature was 60°C. The specific test results are as follows:
[0098]
[0099] The highly dispersed silica obtained in Example 1-3 and Comparative Example 1-2 was used to prepare vulcanized rubber according to the standard of HG / T 2404-2020, and was placed at a temperature of 88°C for 120 hours. After the standing period, the rubber naturally recovered to room temperature, and was immersed in a 24wt% sodium hydroxide solution of 4 times the mass for 72 hours. After the immersion period, the rubber was washed and dried, and the tensile properties were tested again. The test results are as follows:
[0100]
[0101] The invention adopts a specific method to prepare a mixed solution 1, wherein the composite agent as a surfactant can enhance the dispersibility of a sodium silicate solution, so that the mixed solution 1 is more uniform and stable, and can be better in contact with a sulfuric acid solution, so that the reaction is more sufficient, and the silicon dioxide is guaranteed to have a more stable skeleton and a uniform structure, and then the dispersibility of the silicon dioxide is regulated by adjusting the pH in a staged manner, and in the step of preparing primary silicon dioxide, the glyceryl monostearate and polyethylene glycol components can improve the uniform dispersibility of the mixed solution 3, and then vinyl triethoxysilane is added and introduced, which can enhance the hydrophobicity of the silicon dioxide and reduce the aggregation degree, and then thioglycolic acid and ethylenediamine are introduced, wherein the vinyl group can be bonded with the thiol group, and the amino group of the ethylenediamine can form a hydrogen bond with the carboxyl group of the thioglycolic acid, and a stable cross-linking structure is formed therebetween to coat the surface of the silicon dioxide, and combined with high-temperature heat treatment, on the one hand, the dispersibility of the silicon dioxide can be enhanced, the agglomeration between particles is avoided, and the thermal stability is good; on the other hand, the stable cross-linking structure enhances the strength performance and wear resistance of the vulcanized rubber, reduces the loss, and makes the stability of the vulcanized rubber good.
[0102] In comparative example 1, primary silica is obtained by drying mixed solution three, which does not form a stable cross-linked structure on the surface of silica, and the agglomeration force between the obtained silica is strong, and the strength performance is not high, and the stability performance is poor; in comparative example 2, the compounding agent is omitted when preparing mixed solution one, wherein the dispersion performance of the sodium silicate solution is insufficient, and the contact between the sodium silicate solution and the sulfuric acid solution is insufficient, the uniformity of the obtained mixed solution one is poor, the reaction is insufficient, and in the steps of preparing mixed solution two and mixed solution three, the sufficiency of the reaction is further affected, resulting in the obtained silica product having poor morphology, poor hydrophobicity, unstable skeleton, and uneven structure, which affects the dispersion performance of the product, and the loss during heating is large, and the obtained vulcanized rubber has poor strength performance and poor stability performance.
[0103] Unless otherwise specified, all ratios and percentages described in the present invention are by mass ratios and percentages are by mass percentages.
[0104] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing highly dispersed silicon dioxide, characterized in that: The preparation method comprises the steps of preparing a mixed solution 1, preparing a mixed solution 2, preparing a mixed solution 3, preparing primary silicon dioxide, and heat treatment; The step of preparing the mixed solution 1 is to mix the sodium silicate solution and the composite agent, and then heat the mixture to 60-64° C. at a rate of 0.8-1.2° C. / min for ultrasonic treatment, add sulfuric acid solution after the ultrasonic treatment, control the pH value to 4.8-5.2, stir for 12-17 minutes, and stir at a speed of 104-115 rpm. After the stirring is completed, a mixed solution 1 is obtained; The compound is a mixture of sodium citrate, sodium sulfate of fatty alcohol polyoxyethylene ether and Tween 80; The step of preparing the mixed solution II is to add the sodium silicate solution to the mixed solution I, stir evenly, control the addition rate to be 1.0-1.4 mL / min, and the pH value of the system is 8.7-8.9, continue to add the sodium silicate solution, stir evenly, control the addition rate to be 0.7-0.9 mL / min, and the pH value of the system is 11.1-11.5, to obtain the mixed solution II; The step of preparing the mixed solution three is to add sulfuric acid solution to the mixed solution two, stir evenly, control the addition rate to be 1.2-1.4 mL / min, the pH value of the system is 9.6-9.8, continue to add sulfuric acid solution, stir evenly, control the addition rate to be 1.0-1.2 mL / min, the pH value of the system is 8.3-8.7, add sulfuric acid solution again, stir evenly, control the addition rate to be 0.7-0.9 mL / min, the pH value of the system is 7.0, and prepare the mixed solution three; The steps of preparing primary silicon dioxide are as follows: placing the mixed solution in a sealed container, then adding anhydrous ethanol, stirring evenly, adding glyceryl monostearate and polyethylene glycol, and performing ultrasonic treatment. After the ultrasonic treatment, adding vinyl triethoxysilane, heating to 80-84°C at a rate of 0.8-1.2°C / min, reacting for 3.8-4.2h, adding thioglycolic acid and ethylenediamine after the reaction, stirring evenly, controlling the temperature to 34-36°C, performing ultraviolet irradiation, filtering after the irradiation, performing freeze drying, and naturally returning to room temperature after the freezing to obtain primary silicon dioxide.
2. The method for preparing highly dispersed silicon dioxide according to claim 1, characterized in that: In the step of preparing the mixed solution 1, the mass concentration of the sodium silicate solution is 24-28%; The mass ratio of the sodium silicate solution to the composite agent is 24-28:4.5-4.9; The mass concentration of the sulfuric acid solution is 10.2-10.4%.
3. The method for preparing highly dispersed silicon dioxide according to claim 1, characterized in that: In the step of preparing the mixed solution 1, the ultrasonic treatment has an ultrasonic time of 9-12 min, an ultrasonic frequency of 25-30 kHz, and an ultrasonic power of 82-88 W.
4. The method for preparing highly dispersed silicon dioxide according to claim 1, characterized in that: In the composite agent, the mass ratio of the sodium citrate, sodium fatty alcohol polyoxyethylene ether sulfate and Tween 80 is 1.8-2.2:3.2-3.6:2.4-2.
6.
5. The method for preparing highly dispersed silicon dioxide according to claim 1, characterized in that: In the step of preparing the mixed solution 2, the mass concentration of the sodium silicate solution is 24-28%; In the step of preparing the mixed solution three, the mass concentration of the sulfuric acid solution is 10.2-10.4%.
6. The method for preparing highly dispersed silicon dioxide according to claim 1, characterized in that: In the step of preparing primary silicon dioxide, the mass ratio of the mixed solution three, anhydrous ethanol, glyceryl monostearate, polyethylene glycol, vinyl triethoxysilane, thioglycolic acid and ethylenediamine is 18-22:30-34:1.4-1.6:1.1-1.5:1.5-1.7:0.8-1.0:1.1-1.
4.
7. The method for preparing highly dispersed silicon dioxide according to claim 1, characterized in that: In the step of preparing primary silicon dioxide, the ultrasonic treatment has an ultrasonic time of 18-22 min and an ultrasonic power of 116-124 W; The ultraviolet irradiation has an ultraviolet wavelength of 235-245nm and an irradiation time of 1.8-2.2h; The freeze drying has a freezing temperature of -37 to -33°C and a freezing time of 28 to 31 hours.
8. The method for preparing highly dispersed silicon dioxide according to claim 1, characterized in that: The heat treatment step is to place the primary silicon dioxide in a closed environment for heat treatment, firstly heating the temperature to 195-205°C at a rate of 4.8-5.2°C / min, and heat-treating at 195-205°C for 37-43min, then heating the temperature to 354-363°C at a rate of 2.8-3.2°C / min, and heat-treating at 354-363°C for 1.8-2.2h. After the heat-treating is completed, the temperature is naturally lowered to room temperature to obtain highly dispersed silicon dioxide.
Citation Information
Patent Citations
Production method of high-dispersion silicon dioxide
CN114368760A
High-reinforcing and high-dispersion silicon dioxide as well as preparation method and application thereof
CN117735562A
Preparation method of mesoporous silica microsphere
CN108579705A
Preparation method of high-dispersion silicon dioxide suitable for winter tires
CN112390263A
Hydrophobic high-dispersion high-adsorption silicon dioxide for papermaking pigment and preparation method of hydrophobic high-dispersion high-adsorption silicon dioxide
CN114455598A