A low-water absorption ceramic tile sintered at low temperature and a preparation method thereof

By using a combination of zeolite-boric acid intermediate and magnesium soil, potassium sand and sodium sand, the firing temperature of low-water absorption rate ceramic tiles is reduced and the firing temperature range is broadened, and the problems of high firing temperature and long cycle are solved. It realizes the production of low-temperature fast firing and high-performance low-water absorption rate ceramic tiles.

CN118619651BActive Publication Date: 2024-11-08FOSHAN DONGPENG CERAMIC +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411095108.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-08
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

The existing low-water absorption tiles have high firing temperature, narrow firing temperature range and long firing cycle, resulting in high production energy consumption and degradation of tiles.

Method used

Zeolite is used as the adsorbent of nano-scale boric acid to form a zeolite-boric acid intermediate, and dry it at high temperature to form a metaboric acid-zeolite flux, combined with magnesium soil, potassium sand and sodium sand, and is sintered by spray granulation and kiln. , reduce the firing temperature, broaden the temperature range and shorten the firing cycle.

Benefits of technology

The low-temperature and fast firing of low-water absorption tiles is achieved, which reduces production energy consumption, ensures the performance of the tiles, with a water absorption rate of ≤0.04%, and avoids brick deformation and performance degradation caused by excessive liquid phase.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to the technical field of building ceramics, and in particular to a low-water absorption ceramic tile sintered at low temperature and a preparation method thereof, comprising the following steps: A. adding zeolite to a boric acid solution and letting it stand to obtain a zeolite-boric acid intermediate; drying the zeolite-boric acid intermediate at a temperature of 170-190°C to obtain a metaboric acid-zeolite flux; B. preparing a blank raw material, and ball-milling the blank raw material with water, and obtaining a blank after spray granulation; C. pressing the blank, and firing it in a kiln to obtain a low-water absorption ceramic tile; wherein the firing temperature of the low-water absorption ceramic tile is 1060-1070°C, and the firing cycle is 35-38min. The preparation method of a low-water absorption ceramic tile sintered at low temperature proposed by the present invention realizes the low-temperature fast firing of the low-water absorption ceramic tile under the premise of reducing the addition amount of fluxing components in the formula, reducing the amount of liquid phase, and ensuring the performance of the ceramic tile, thereby effectively reducing the production energy consumption of the low-water absorption ceramic tile.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building ceramics, and in particular to a low-water absorption ceramic tile sintered at a low temperature and a preparation method thereof. Background Art

[0002] In building ceramic technology, reducing firing energy consumption is an important part of reducing production costs and improving economic benefits; and the fundamental way to reduce the firing temperature of tiles is to achieve low-temperature firing of tiles. The firing temperature of existing low-water absorption tiles (referring to tiles with a water absorption rate of ≤0.5%) is generally between 1180 and 1250°C, which not only consumes a lot of energy and minerals, but also makes the production cost of tiles relatively high.

[0003] In order to reduce the firing temperature of ceramic tiles, the prior art generally adopts the method of introducing low-temperature sand containing K2O and Na2O, so that the ceramic tile body can be sintered in advance before the temperature reaches the lowest eutectic point, thereby achieving the purpose of low-temperature sintering. However, before the temperature reaches the lowest eutectic point, the amount of liquid phase that appears is very small. However, when the temperature reaches the lowest eutectic point, a large amount of liquid phase will appear immediately, and it will increase rapidly with the increase of temperature, causing the ceramic tile body to deform. Therefore, although the method of introducing low-temperature sand can reduce the sintering temperature of ceramic tiles, it will also narrow the firing temperature range of ceramic tiles. In addition, if the firing temperature range of ceramic tiles is too narrow, it is easy to cause the ceramic tiles to be under-fired, resulting in insufficient densification of the ceramic tiles; or it is easy to cause the ceramic tiles to be over-fired, resulting in easy deformation of the ceramic tiles, resulting in bending and warping, and uneven brick bodies, which will affect the decline of the overall performance indicators of the ceramic tiles (such as strength and other properties).

[0004] In order to overcome the above defects, the industry has developed a method of wrapping the green body powder with a low-temperature sintering mineralizing liquid containing boron to form a quaternary composite flux of K2O-Na2O-MgO-B2O3, so that the amount of liquid phase generated under the action of the quaternary composite flux gradually increases, and gradually appears in the tile green body in a step-by-step manner, and gradually dissolves other substances, making the tile more compact, thereby achieving the purpose of lowering the firing temperature, widening the firing temperature range, and shortening the firing cycle. However, the above-mentioned quaternary composite flux easily generates a large amount of liquid phase in the tile green body, and when the amount of liquid phase in the green body is too much, liquid phase will exist between the solid phase particles that act as the skeleton of the tile, which will reduce the friction between the solid phase particles and easily cause displacement, which will cause the tile body to be easily deformed and uneven, and also reduce the overall performance indicators of the tile. Summary of the invention

[0005] The purpose of the present invention is to propose a method for preparing low-temperature sintered low-water absorption ceramic tiles, which is beneficial to reduce the amount of fluxing components added in the formula, reduce the amount of liquid phase, and ensure the performance of the ceramic tiles. It overcomes the defects of high firing temperature, narrow firing temperature range and long firing cycle of low-water absorption ceramic tiles in the prior art, realizes low-temperature and fast firing of low-water absorption ceramic tiles, thereby effectively reducing the production energy consumption of low-water absorption ceramic tiles.

[0006] Another object of the present invention is to propose a low-temperature sintered, low-water absorption ceramic tile prepared by the above-mentioned preparation method, which can effectively reduce the firing temperature of the ceramic tile, broaden its firing temperature range and shorten its firing cycle while reducing the amount of fluxing components added in the formula, reducing the amount of liquid phase and ensuring the performance of the ceramic tile, so as to achieve low-temperature firing of ceramic tiles with a water absorption rate of less than 0.04%, thereby overcoming the shortcomings of the prior art.

[0007] To achieve this object, the present invention adopts the following technical solutions:

[0008] A method for preparing low-temperature sintered low-water absorption ceramic tiles comprises the following steps:

[0009] A. adding zeolite to a boric acid solution and letting it stand to obtain a zeolite-boric acid intermediate; drying the zeolite-boric acid intermediate at a temperature of 170 to 190° C. to obtain a metaboric acid-zeolite flux;

[0010] B. preparing a raw material for a green body, and ball-milling the raw material for the green body with water, and obtaining a green body after spray granulation; wherein, calculated by mass percentage, the raw material for the green body comprises: 6-16% of metaboric acid-zeolite flux, 13-17% of bauxite, 10-16% of magnesia clay, 10-15% of potassium sand, 16-18% of sodium sand, 10-23% of mixed mud, and 12-18% of bentonite;

[0011] C. After the blank is pressed, it is put into a kiln for firing to obtain low water absorption ceramic tiles; wherein the firing temperature of the low water absorption ceramic tiles is 1060-1070°C, and the firing cycle is 35-38 minutes.

[0012] Furthermore, in step A, the mesh size of the zeolite is 60 to 200 meshes.

[0013] Furthermore, in step A, the boric acid solution includes boric acid and water, and calculated by mass ratio, the mixing ratio of the boric acid to the water is (5-7):100.

[0014] Furthermore, in step A, the standing time is 2 to 3 days, and the mixing ratio of the zeolite and the boric acid solution is (2 to 3):25 calculated by mass ratio.

[0015] Furthermore, in step B, calculated by mass percentage, the green body raw materials include: 12% metaboric acid-zeolite flux, 15% bauxite, 13% magnesia clay, 15% potassium sand, 17% sodium sand, 14% mixed mud and 14% bentonite.

[0016] Furthermore, calculated by mass percentage, the chemical composition of the potash sand includes MgO 0.10-0.15%, CaO 0.30-0.40%, Al2O3 17.10-17.30%, SiO2 71.40-71.60%, K2O 3.90-4.00%, Na20 0.50-0.60%, TiO2 0.12-0.15% and Fe2O3 1.60-1.70%, and the rest is loss on ignition.

[0017] Furthermore, calculated by mass percentage, the chemical composition of the sodium sand includes MgO 0.15-0.20%, CaO 0.05-0.10%, Al2O3 17.10-17.30%, SiO2 71.20-71.40%, K2O 1.30-1.40%, Na20 4.50-4.60%, TiO2 0.05-0.10% and Fe2O3 0.90-1.00%, and the rest is loss on ignition.

[0018] Furthermore, calculated by mass percentage, the chemical composition of the magnesia soil includes MgO 10-15%, CaO 7.10-7.40%, Al2O3 18.60-18.80%, SiO2 47.60-47.90%, K2O 0.30-0.40%, Na20 0.40-0.60%, TiO2 0.10-0.20% and Fe2O3 1.45-1.60%, and the rest is loss on ignition.

[0019] Furthermore, calculated by mass percentage, the chemical composition of the mixed mud includes MgO 0.50-0.70%, CaO 0.80-0.90%, Al2O3 24.20-24.40%, SiO2 63.50-63.90%, K2O 1.30-1.40%, Na20 0.10-0.30%, TiO2 0.20-0.40% and Fe2O3 1.10-1.20%, and the rest is loss on ignition.

[0020] A low-water absorption ceramic tile sintered at a low temperature is prepared using the above-mentioned preparation method of the low-water absorption ceramic tile sintered at a low temperature, and the water absorption of the low-water absorption ceramic tile is 0.02-0.04%.

[0021] The technical solution provided by the present invention may include the following beneficial effects:

[0022] 1. Zeolite is used as an adsorbent of nano-boric acid to form a zeolite-boric acid intermediate, and then the zeolite-boric acid intermediate is dried at high temperature, so that the nano-boric acid is decomposed into nano-boric acid that is not easily soluble in water and exists inside the zeolite, forming a metaboric acid-zeolite flux. Based on the composition and structure of zeolite itself and the characteristics of the large specific surface area of ​​nano-boric acid, boron trioxide is introduced into the formula in the form of metaboric acid-zeolite flux, and the contact area between boron trioxide and the raw materials forming the solid phase in the formula is very large, which can accelerate the dissolution-precipitation mass transfer process, promote the rearrangement and densification between the solid phase particles, and accelerate the sintering process, so as to facilitate the fluxing components in the formula, metaboric acid-zeolite flux, magnesia soil, potassium sand and sodium sand, when the addition amount is as low as 42-65%, it can also achieve the purpose of reducing the firing temperature, widening the firing temperature range and shortening the firing cycle.

[0023] 2. Since the amount of fluxing component added in the formula is small, it is beneficial to reduce the amount of liquid phase produced during the calcination process, avoiding excessive liquid phase, which reduces the friction between solid particles and easily causes displacement, causing the tile body to be easily deformed, resulting in bending and warping, and uneven brick body, affecting the strength and other properties of the tile, thereby ensuring the performance of the tile. DETAILED DESCRIPTION

[0024] The present technical solution provides a method for preparing low-water absorption ceramic tiles sintered at low temperature, comprising the following steps:

[0025] A. adding zeolite to a boric acid solution and letting it stand to obtain a zeolite-boric acid intermediate; drying the zeolite-boric acid intermediate at a temperature of 170 to 190° C. to obtain a metaboric acid-zeolite flux;

[0026] B. preparing a raw material for a green body, and ball-milling the raw material for the green body with water, and obtaining a green body after spray granulation; wherein, calculated by mass percentage, the raw material for the green body comprises: 6-16% of metaboric acid-zeolite flux, 13-17% of bauxite, 10-16% of magnesia clay, 10-15% of potassium sand, 16-18% of sodium sand, 10-23% of mixed mud, and 12-18% of bentonite;

[0027] C. After the blank is pressed, it is put into a kiln for firing to obtain low water absorption ceramic tiles; wherein the firing temperature of the low water absorption ceramic tiles is 1060-1070°C, and the firing cycle is 35-38 minutes.

[0028] In the prior art, the green body powder is wrapped with a low-temperature sintering mineralization liquid containing boron to form a quaternary composite flux of K2O-Na2O-MgO-B2O3, but the quaternary composite flux generates a large amount of liquid phase in the tile. When there is too much liquid phase in the tile, liquid phase exists between the solid phase particles that serve as the skeleton of the tile, which reduces the friction between the solid phase particles and easily causes displacement, which in turn causes the tile to deform easily, resulting in bending and warping, and uneven brick body, which also reduces the overall performance indicators of the tile.

[0029] In order to solve the defects of low water absorption ceramic tiles in the prior art, such as high firing temperature, narrow firing temperature range and long firing cycle, the present technical scheme proposes a method for preparing low water absorption ceramic tiles sintered at low temperature, using zeolite as an adsorbent for nano-boric acid to form a zeolite-boric acid intermediate, and then drying the zeolite-boric acid intermediate at high temperature, so that the nano-boric acid is decomposed into nano-metaboric acid that is not easily soluble in water and exists inside the zeolite, forming a metaboric acid-zeolite flux. Based on the composition and structure of zeolite itself and the large specific surface area of ​​nano-scale metaboric acid, boron trioxide is introduced into the formula in the form of metaboric acid-zeolite flux, and the contact area between boron trioxide and the raw materials forming the solid phase in the formula is very large, which can accelerate the dissolution-precipitation mass transfer process, promote the rearrangement and densification between solid phase particles, and accelerate the sintering process, so that the fluxing components metaboric acid-zeolite flux, magnesia clay, potassium sand and sodium sand in the formula can also achieve the purpose of reducing the firing temperature, widening the firing temperature range and shortening the firing cycle when the addition amount is as low as 42-65%. In addition, since the addition amount of fluxing components in the formula is small, it is beneficial to reduce the amount of liquid phase generated during the calcination process, avoiding excessive liquid phase, resulting in reduced friction between solid phase particles and easy displacement, causing the tile body to be easily deformed, resulting in bending and warping, uneven brick body, affecting the strength of the tile, etc., thereby ensuring the performance of the tile.

[0030] Specifically, zeolite is a porous aluminosilicate crystal with a large number of pores with a pore size of 0.3 to 1 nm. Boric acid is easily hydrolyzed to generate H in an aqueous environment. + Ions and B(OH)4 - ions, therefore, the technical solution first adds zeolite into the boric acid solution and allows it to stand, and due to B (OH) 4 - The diameter of the ion is 0.284 nm, which is smaller than the pore size of zeolite, making B(OH)4 - It can easily enter the pores by diffusion. In addition, the interior of the zeolite contains a large number of positive ions and exchangeable positive ion vacancies, making B (OH) 4 - Ions can be adsorbed into the interior of zeolite through electrostatic adsorption. +Ions enter the zeolite through ion exchange. That is, the boric acid molecules in the boric acid solution can enter the zeolite through electrostatic adsorption, ion exchange, diffusion and other interactions, and due to the pore size characteristics and molecular sieve effect of the zeolite, the boric acid molecules exist in the zeolite in the form of nano-sized boric acid molecules. It should be noted that the pore size characteristics enable zeolite to distinguish and adsorb molecules according to the size or geometric shape of different molecules, forming a molecular sieve effect.

[0031] Secondly, boron exists in nature mainly in the form of boric acid and borate, while boric acid is widely used in the metallurgical field, and borate, such as borax, is widely used in the ceramic field. Since both boric acid and borax are soluble in water and volatilize during the spray granulation process, it is impossible to use boric acid and borax as raw materials for the green body in the process of preparing ceramic green bodies by wet powder making process. The decomposition temperature of boric acid is 169°C. The technical solution dries the zeolite-boric acid intermediate at a temperature of 170-190°C, so that the nano-boric acid in the zeolite-boric acid intermediate decomposes into nano-boric acid insoluble in water at this drying temperature, thereby forming a metaboric acid-zeolite flux, avoiding the volatilization of boric acid in the spray granulation process, so that the boric acid widely used in the metallurgical field can be directly used in the preparation of tiles in the ceramic field.

[0032] Secondly, the metaboric acid-zeolite flux is broken during the spray granulation process, so that the nano-scale metaboric acid inside the metaboric acid-zeolite flux is directly exposed, and during the kiln calcination process, the nano-scale metaboric acid is dehydrated to generate boron trioxide with a strong fluxing effect, which is beneficial to reduce the firing temperature of tiles and increase the firing temperature range. At the same time, during the spray granulation process, based on the composition and structure of the zeolite itself, compared with potassium and sodium feldspar, the metaboric acid-zeolite flux is easier to be broken, making the nano-scale metaboric acid inside the metaboric acid-zeolite flux easier to be directly exposed, which is more conducive to achieving the purpose of reducing the firing temperature, widening the firing temperature range and shortening the firing cycle. In addition, since nano-level metaboric acid exists in the form of metaboric acid-zeolite flux, on the one hand, metaboric acid-zeolite flux is conducive to the full dispersion of nano-level metaboric acid in the formula, increasing the contact area with the high-temperature raw materials (i.e., raw materials forming the solid phase) in the formula; on the other hand, since the particles of nano-level metaboric acid itself are extremely small, its specific surface area is extremely large, which is also conducive to increasing the contact area with the raw materials forming the solid phase in the formula. Through the mutual coordination of the two, the contact area between the nano-level metaboric acid in the form of metaboric acid-zeolite flux and the raw materials forming the solid phase in the formula is greatly improved, so that the boron trioxide obtained by calcining nano-level metaboric acid in the kiln can form a liquid phase at a lower temperature that can be more widely distributed in the ceramic tile body, and the liquid phase as a medium in the sintering process can accelerate the mass transfer process, promote the rearrangement and densification between the solid phase particles, accelerate the sintering process, and is more conducive to shortening the sintering time, reducing energy consumption, and improving production efficiency. That is, based on the fact that the metaboric acid-zeolite flux is easy to break and the increase in the contact area between the metaboric acid-zeolite flux and the raw materials forming the solid phase, the above two aspects cooperate with each other to enable the metaboric acid-zeolite flux to act as a strong flux, greatly reducing the firing temperature, widening the firing temperature range and shortening the firing cycle.

[0033] It should be noted that the B(OH)4 - The dispersion of ions is uniform, which is conducive to avoiding the technical defects of easily causing uneven sintering degree and bringing performance degradation such as strength when directly using boric acid as the raw material of the green body. In addition, in the present technical solution, the metaboric acid-zeolite flux is actually a particle formed by the combination of nano-level metaboric acid and zeolite, and its particle size is larger than that of metaboric acid. If the nano-level metaboric acid or nano-level boric oxide equivalent to the metaboric acid particle size is directly added to the green body raw material, it will cause the particle size of some particles to be too small, and the matching property with the remaining raw materials in the green body raw material is poor, so that the green body obtained by pressing is prone to delamination and cracking, affecting the performance of ceramic tile, therefore, the nano-level metaboric acid or nano-level boric oxide equivalent to the metaboric acid particle size cannot be directly added in the present technical solution.

[0034] It should be further explained that the flux in the present technical solution includes two categories. The first category is magnesia clay, potassium sand and sodium sand. Among them, magnesia clay provides magnesium oxide, which is beneficial to reduce the viscosity of the melt formed after the raw materials are calcined, and adjust the chemical stability of the melt. Potassium sand and sodium sand are both used to provide potassium oxide and sodium oxide. Potassium oxide and sodium oxide can form ionic bonds in the melt to reduce the viscosity of the melt. Therefore, in the present technical solution, by introducing three raw materials, magnesia clay, potassium sand and sodium sand, and limiting their addition amounts, it is beneficial to form fluxes with different temperature gradients, thereby ensuring that the melt formed after calcination always has chemical properties and suitable viscosity as the temperature rises, thereby ensuring the performance of the tile. The second largest category is metaboric acid-zeolite flux. The metaboric acid in the metaboric acid-zeolite flux is nanometer-grade, and its contact area with the raw materials that form the solid phase in the formula, such as mixed mud, bentonite and bauxite, is greatly improved, ensuring that adding 6-16% of metaboric acid-zeolite flux to the formula can achieve a good fluxing effect. While reducing the use of fluxing components, reducing the generation of liquid phase, and ensuring the performance of tiles, it can not only ensure that the firing temperature is lowered, the firing temperature range is widened, and the firing cycle is shortened, but it is also beneficial to avoid the technical defects of directly using boric acid as a green body raw material, which is easy to cause uneven sintering and bring about a decrease in the strength of the tiles and other performance.

[0035] Further, in step A, the mesh size of the zeolite is 60 to 200 meshes.

[0036] When the mesh number of zeolite particles is less than 60 meshes, the particles are relatively large, and the contact area between zeolite and boric acid dissolution will be reduced. The reduction in contact area will lead to a corresponding decrease in the electrostatic adsorption and ion exchange effects of zeolite particles on boric acid, resulting in a decrease in the amount of metaboric acid in the metaboric acid-zeolite flux, thereby reducing the fluxing effect of the metaboric acid-zeolite flux. When the mesh number of zeolite particles is greater than 200 meshes, the particles of the obtained metaboric acid-zeolite flux will be too small, and the particles will be further refined during the ball milling process, resulting in a weaker bonding force between the metaboric acid-zeolite flux and other raw materials in the green body formed by pressing the green body, making the green body prone to defects such as cracking and delamination, thereby affecting the performance of the tile.

[0037] Further, in step A, the boric acid solution includes boric acid and water, and calculated by mass ratio, the mixing ratio of the boric acid to the water is (5-7):100.

[0038] The technical solution preferably has a mixing ratio of boric acid to water of (5-7):100, which ensures that the boric acid can be completely dissolved and reaches the dissolution saturation at a relatively low cost, and ensures that the fluxing effect of the metaboric acid-zeolite flux is optimal, thereby ensuring the performance of the tile.

[0039] Further, in step A, the standing time is 2 to 3 days, and the mixing ratio of the zeolite and the boric acid solution is (2 to 3):25 calculated by mass ratio.

[0040] The technical solution optimizes the standing time and the mixing ratio of zeolite and boric acid solution, which is more conducive to the boric acid in the boric acid solution to completely enter the interior of the zeolite and diffuse inside the zeolite to be further dispersed, thereby being more conducive to ensuring the fluxing performance of the metaboric acid-zeolite flux.

[0041] Further explanation, in step B, calculated by mass percentage, the green body raw materials include: 12% metaboric acid-zeolite flux, 15% bauxite, 13% magnesia clay, 15% potassium sand, 17% sodium sand, 14% mixed mud and 14% bentonite.

[0042] This technical solution ensures that the performance of the obtained tiles reaches the best by further optimizing the addition amount of the blank raw materials.

[0043] It is further explained that, calculated by mass percentage, the chemical composition of the potash sand includes MgO 0.10-0.15%, CaO 0.30-0.40%, Al2O3 17.10-17.30%, SiO2 71.40-71.60%, K2O 3.90-4.00%, Na20 0.50-0.60%, TiO2 0.12-0.15% and Fe2O3 1.60-1.70%, and the rest is loss on ignition.

[0044] The technical solution preferably adds potassium sand with a K2O content of 3.90-4.00% calculated by mass percentage to the green body raw material, which helps to increase the K2O content in the formula, so as to achieve the purpose of reducing the firing temperature, widening the firing temperature range and shortening the firing cycle. At the same time, the SiO2 content in potassium sand is as high as more than 70%, and the Al2O3 content is as high as 17%, which is conducive to increasing the content of silicon and aluminum in the formula, and improving the mechanical properties of tiles while ensuring the fluxing effect of potassium sand.

[0045] It is further explained that, calculated by mass percentage, the chemical composition of the sodium sand includes MgO 0.15-0.20%, CaO 0.05-0.10%, Al2O3 17.10-17.30%, SiO2 71.20-71.40%, K2O 1.30-1.40%, Na20 4.50-4.60%, TiO2 0.05-0.10% and Fe2O3 0.90-1.00%, and the rest is loss on ignition.

[0046] The technical solution preferably adds sodium sand with a Na2O content of 4.50-4.60% calculated by mass percentage to the green body raw material, which helps to increase the Na2O content in the formula, so as to achieve the purpose of reducing the firing temperature, widening the firing temperature range and shortening the firing cycle. At the same time, the SiO2 content in the sodium sand is as high as more than 70%, and the Al2O3 content is as high as 17%, which is conducive to increasing the content of silicon and aluminum in the formula, and improving the mechanical properties of the tile while ensuring the sodium sand fluxing effect.

[0047] It is further explained that, calculated by mass percentage, the chemical composition of the magnesia soil includes MgO 10-15%, CaO 7.10-7.40%, Al2O3 18.60-18.80%, SiO2 47.60-47.90%, K2O 0.30-0.40%, Na20 0.40-0.60%, TiO2 0.10-0.20% and Fe2O3 1.45-1.60%, and the rest is loss on ignition.

[0048] The technical solution preferably adds magnesia clay with a MgO content of 10-15% and a CaO content of 7.10-7.40% calculated by mass percentage to the green body raw material, which helps to increase the content of MgO and CaO in the formula, so as to achieve the purpose of lowering the firing temperature, widening the firing temperature range and shortening the firing cycle.

[0049] It is further explained that, calculated by mass percentage, the chemical composition of the mixed mud includes MgO 0.50-0.70%, CaO 0.80-0.90%, Al2O3 24.20-24.40%, SiO2 63.50-63.90%, K2O 1.30-1.40%, Na20 0.10-0.30%, TiO2 0.20-0.40% and Fe2O3 1.10-1.20%, and the rest is loss on ignition.

[0050] The technical solution preferably adds a mixed mud with a SiO2 content of 63.50-63.90% and an Al2O3 content of 24.20-24.40% calculated by mass percentage to the green body raw material, which is beneficial to increase the silicon and aluminum content in the formula and improve the mechanical properties of the tile.

[0051] A low-water absorption ceramic tile sintered at a low temperature is prepared using the above-mentioned preparation method of the low-water absorption ceramic tile sintered at a low temperature, and the water absorption of the low-water absorption ceramic tile is 0.02-0.04%.

[0052] The low water absorption ceramic tile prepared by the above-mentioned preparation method proposed in this scheme can effectively reduce the firing temperature of the ceramic tile, broaden its firing temperature range and shorten its firing cycle, so as to achieve low-temperature firing of ceramic tiles with a water absorption rate of less than 0.04%.

[0053] The technical solution of the present invention is further illustrated below through specific implementation methods.

[0054] In the embodiments and comparative examples of the present invention, the chemical composition of potash sand includes MgO 0.13%, CaO 0.32%, Al2O3 17.10%, SiO2 71.50%, K2O 3.95%, Na2O 0.54%, TiO2 0.13% and Fe2O3 1.67%, and the rest is loss on ignition; the chemical composition of sodium sand includes MgO 0.19%, CaO 0.05-0.10%, Al2O3 17.20%, SiO2 71.22%, K2O 1.35%, Na2O 4.55%, TiO2 0.06% and Fe2O3 0.94%, and the rest is loss on ignition; the chemical composition of magnesia soil includes MgO 12.13%, CaO 7.30%, Al2O3 18.72%, SiO2 47.68%, K2O 0.23%, Na2O 0.41%, TiO2 0.05% and Fe2O3 1.58%, and the rest is loss on ignition; calculated by mass percentage, the chemical composition of the mixed mud includes MgO 0.67%, CaO 0.81%, Al2O3 24.32%, SiO2 63.83%, K2O 1.39%, Na2O 0.23%, TiO2 0.30% and Fe2O3 1.13%, and the rest is loss on ignition, and the rest is loss on ignition. In addition, if the specific technology or conditions are not specified in the embodiments and comparative examples, the technology or conditions described in the literature in this field or the product manual shall be followed. The reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased commercially.

[0055] Example 1

[0056] A. adding 10 g of zeolite with a mesh size of 100 meshes into 100 g of boric acid solution and leaving the mixture to stand for 2 days to obtain a zeolite-boric acid intermediate; drying the zeolite-boric acid intermediate at a temperature of 170° C. to obtain a metaboric acid-zeolite flux; wherein the boric acid solution comprises boric acid and water, and the mixing ratio of boric acid to water is 5:100 calculated by mass ratio;

[0057] B. preparing a green body raw material, adding water to the green body raw material and ball milling the green body raw material, and obtaining a green body after spray granulation; wherein, calculated by mass percentage, the green body raw material comprises: 12% of metaboric acid-zeolite flux, 15% of bauxite, 13% of magnesia clay, 15% of potassium sand, 17% of sodium sand, 14% of mixed mud and 14% of bentonite;

[0058] C. After the blank is pressed, it is put into a kiln for firing to obtain low water absorption ceramic tiles; wherein, the firing temperature of the low water absorption ceramic tiles is 1060°C, and the firing cycle is 38 minutes.

[0059] Example 2

[0060] A. adding 8 g of zeolite with a mesh number of 120 into 100 g of boric acid solution and letting it stand for 2 days to obtain a zeolite-boric acid intermediate; drying the zeolite-boric acid intermediate at a temperature of 180° C. to obtain a metaboric acid-zeolite flux; wherein the boric acid solution comprises boric acid and water, and the mixing ratio of boric acid to water is 5:100 calculated by mass ratio;

[0061] B. preparing a green body raw material, adding water to the green body raw material and ball milling the green body raw material, and obtaining a green body after spray granulation; wherein, calculated by mass percentage, the green body raw material includes: 6% of metaboric acid-zeolite flux, 17% of bauxite, 16% of magnesia clay, 15% of potassium sand, 18% of sodium sand, 10% of mixed mud and 18% of bentonite;

[0062] C. After the blank is pressed, it is put into a kiln for firing to obtain low water absorption ceramic tiles; wherein, the firing temperature of the low water absorption ceramic tiles is 1070°C, and the firing cycle is 35 minutes.

[0063] Example 3

[0064] A. adding 12 g of zeolite with a mesh number of 60 into 100 g of boric acid solution and letting it stand for 3 days to obtain a zeolite-boric acid intermediate; drying the zeolite-boric acid intermediate at a temperature of 190° C. to obtain a metaboric acid-zeolite flux; wherein the boric acid solution comprises boric acid and water, and the mixing ratio of boric acid to water is 6:100 calculated by mass ratio;

[0065] B. preparing a green body raw material, adding water to the green body raw material and ball milling the green body raw material, and obtaining a green body after spray granulation; wherein, calculated by mass percentage, the green body raw material includes: 16% of metaboric acid-zeolite flux, 10% of bauxite, 10% of magnesia clay, 12% of potassium sand, 16% of sodium sand, 23% of mixed mud and 13% of bentonite;

[0066] C. After the blank is pressed, it is put into a kiln for firing to obtain low water absorption ceramic tiles; wherein, the firing temperature of the low water absorption ceramic tiles is 1065°C, and the firing cycle is 36 minutes.

[0067] Comparative Example 1

[0068] A. Prepare green body raw materials; at the same time, dissolve 5 parts of boric acid in 95 parts of water at a temperature of 60°C according to the mass ratio to obtain a low-temperature sintering mineralization liquid;

[0069] Among them, the raw materials of the green body are composed of the following raw materials in terms of mass: 15 parts of magnesia clay, 6 parts of bauxite, 1 part of bentonite, 5 parts of mixed mud, 12 parts of potassium-sodium feldspar, 32 parts of potassium-sodium sand and 10 parts of potassium sand;

[0070] B. Add water to the green body raw material and ball grind it, remove iron and spray granulate it to obtain powder, then evenly spray the low-temperature sintering mineralization liquid on the surface of the powder to obtain the green body; wherein, according to the mass ratio, the mixing ratio of the powder and the low-temperature sintering mineralization liquid is 100:6;

[0071] C. After the blank is pressed, it is put into a kiln for firing to obtain low water absorption ceramic tiles; wherein, the firing temperature of the low water absorption ceramic tiles is 1060°C, and the firing cycle is 38 minutes.

[0072] Comparative Example 2

[0073] The preparation method and raw materials of Comparative Example 2 are the same as those of Example 1, except that no metaboric acid-zeolite flux is added to the blank raw material formula in Comparative Example 2, that is, in Comparative Example 2, calculated by mass percentage, the blank raw materials include the following raw materials: 16% bauxite, 15% magnesia clay, 15% potassium sand, 17% sodium sand, 14% mixed mud and 23% bentonite.

[0074] Comparative Example 3

[0075] The preparation method and raw materials of Comparative Example 3 are the same as those of Example 1, except that boric acid is used in the green body raw material in Comparative Example 3 instead of metaboric acid-zeolite flux.

[0076] According to the preparation methods in Examples 1-3 and Comparative Examples 1-3, low water absorption ceramic tiles were prepared, and the raw materials and process parameters not mentioned in the steps of Examples 1-3 were ensured to be consistent. The morphology and surface effect of the green body were observed. The low water absorption ceramic tiles in the above Examples and Comparative Examples were subjected to conventional water absorption, breaking strength and rupture modulus tests in the ceramic field. The performance test results are shown in Table 1 below:

[0077] Table 1 Performance test results of different tiles in the examples and comparative examples

[0078]

[0079] From the performance test results of each embodiment in the above table, it can be seen that the low water absorption ceramic tile prepared by the preparation method of this scheme has no deformation and a smooth surface. It can be fired under the firing conditions of a firing temperature of 1060-1070°C and a firing cycle of 35-38min. The water absorption of the prepared ceramic tile is less than 0.04%, which is lower than that of conventional low water absorption ceramic tiles (water absorption ≤0.5%). The modulus of rupture is ≥52MPa, the destructive strength is ≥2300N, and the mechanical strength is good.

[0080] In Comparative Example 1, due to the excessive addition of fluxing components, the amount of liquid phase formed during the firing process of the green body obtained by pressing the green body raw materials is too large, resulting in deformation of the calcined tile body, unevenness of the tile body, and reduced strength.

[0081] In Comparative Example 2, since no metaboric acid-zeolite flux was added, the green body obtained by pressing the green body raw materials could not be fired, the surface of the obtained tile was uneven, and the water absorption rate of the tile increased and the strength decreased.

[0082] In Comparative Example 3, since boric acid is used instead of metaboric acid-zeolite flux, it is easy to cause uneven sintering and reduce the strength of the tile. At the same time, boric acid volatilizes during the spray granulation process, resulting in its inability to exert its performance. In addition, compared with the introduction of boron element by metaboric acid-zeolite flux, the contact area between the boron element introduced by boric acid and the raw materials forming the solid phase in the formula is reduced. The superposition of the above two factors leads to the inability to burn the green body obtained by pressing the green body raw materials, and the surface of the obtained tile is uneven, and the water absorption rate of the tile increases, and the strength is further reduced.

[0083] The technical principle of the present invention is described above in conjunction with specific embodiments. These descriptions are only for explaining the principle of the present invention and cannot be interpreted as limiting the scope of protection of the present invention in any way. Based on the explanations herein, those skilled in the art can associate other specific implementations of the present invention without paying creative labor, and these methods will fall within the scope of protection of the present invention.

Claims

1. A method for preparing low-temperature sintered low-water absorption ceramic tiles, characterized in that: The following steps are involved: A. adding zeolite to a boric acid solution and letting it stand to obtain a zeolite-boric acid intermediate; drying the zeolite-boric acid intermediate at a temperature of 170 to 190° C. to obtain a metaboric acid-zeolite flux; B. preparing a raw material for a green body, and ball-milling the raw material for the green body with water, and obtaining a green body after spray granulation; wherein, calculated by mass percentage, the raw material for the green body comprises: 6-16% of metaboric acid-zeolite flux, 13-17% of bauxite, 10-16% of magnesia clay, 10-15% of potassium sand, 16-18% of sodium sand, 10-23% of mixed mud, and 12-18% of bentonite; C. After the blank is pressed, it is put into a kiln for firing to obtain low water absorption ceramic tiles; wherein the firing temperature of the low water absorption ceramic tiles is 1060-1070°C, and the firing cycle is 35-38 minutes.

2. The method for preparing a low-temperature sintered low water absorption ceramic tile according to claim 1, characterized in that: In step A, the mesh size of the zeolite is 60 to 200 meshes.

3. The method for preparing a low-temperature sintered low-water absorption ceramic tile according to claim 1, characterized in that: In step A, the boric acid solution includes boric acid and water, and calculated by mass ratio, the mixing ratio of the boric acid to the water is (5-7):

100.

4. The method for preparing a low-temperature sintered low water absorption ceramic tile according to claim 1, characterized in that: In step A, the standing time is 2 to 3 days, and the mixing ratio of the zeolite and the boric acid solution is (2 to 3):25 calculated by mass ratio.

5. The method for preparing a low-temperature sintered low-water absorption ceramic tile according to claim 1, characterized in that: In step B, calculated by mass percentage, the green body raw materials include: 12% metaboric acid-zeolite flux, 15% bauxite, 13% magnesia clay, 15% potassium sand, 17% sodium sand, 14% mixed mud and 14% bentonite.

6. The method for preparing a low-temperature sintered low-water absorption ceramic tile according to claim 1, characterized in that: Calculated by mass percentage, the chemical composition of the potash sand includes MgO 0.10-0.15%, CaO 0.30-0.40%, Al2O3 17.10-17.30%, SiO2 71.40-71.60%, K2O 3.90-4.00%, Na20 0.50-0.60%, TiO2 0.12-0.15% and Fe2O3 1.60-1.70%, and the rest is loss on ignition.

7. The method for preparing a low-temperature sintered low water absorption ceramic tile according to claim 1, characterized in that: Calculated by mass percentage, the chemical composition of the sodium sand includes MgO 0.15-0.20%, CaO 0.05-0.10%, Al2O3 17.10-17.30%, SiO2 71.20-71.40%, K2O 1.30-1.40%, Na20 4.50-4.60%, TiO2 0.05-0.10% and Fe2O3 0.90-1.00%, and the rest is loss on ignition.

8. The method for preparing a low-temperature sintered low water absorption ceramic tile according to claim 1, characterized in that: Calculated by mass percentage, the chemical composition of the magnesia soil includes MgO 10-15%, CaO 7.10-7.40%, Al2O3 18.60-18.80%, SiO2 47.60-47.90%, K2O 0.30-0.40%, Na20 0.40-0.60%, TiO2 0.10-0.20% and Fe2O3 1.45-1.60%, and the rest is loss on ignition.

9. The method for preparing a low-temperature sintered low water absorption ceramic tile according to claim 1, characterized in that: Calculated by mass percentage, the chemical composition of the mixed mud includes MgO 0.50-0.70%, CaO 0.80-0.90%, Al2O3 24.20-24.40%, SiO2 63.50-63.90%, K2O 1.30-1.40%, Na20 0.10-0.30%, TiO2 0.20-0.40% and Fe2O3 1.10-1.20%, and the rest is loss on ignition.

10. A low-temperature sintered low-water absorption ceramic tile, characterized in that: The low water absorption ceramic tile is prepared by the method for preparing low temperature sintered ceramic tiles according to any one of claims 1 to 9, wherein the water absorption of the low water absorption ceramic tile is 0.02 to 0.04%.