Cationic polymer suitable for dehydration of chemical sludge and preparation method thereof
By using nano-chitosan and cationic polymers prepared by copolymerization of cationic monomers in chemical sludge dehydration, combined with destabilizing agents and conditioning agents, the problems of high moisture content and low filtrate turbidity removal rate in chemical sludge dehydration are solved. Achieving more efficient dehydration and flocculation effects.
Patent Information
- Application Number
- CN202411103023.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-08-13
AI Technical Summary
During the dehydration process of chemical sludge, there are problems such as high moisture content, low filtrate turbidity removal rate and difficulty in dehydration. The flocculants in the existing technology have high filter cake moisture content and low filtrate turbidity removal rate during chemical sludge dehydration. The efficiency is low and dehydration is difficult during the filter press process.
A cationic polymer prepared through a copolymerization process using nanochitosan, cationic monomers, acrylamide, and micro-cross-linking agents. Destabilizing agents and conditioning agents are introduced to form a network structure and micro-cross-linking network to enhance electrical neutralization and coiling. The sweeping ability breaks the balance structure of sludge suspended solids, forms dense flocs, and reduces the moisture content of the filter cake.
It significantly reduces the moisture content of the filter cake and improves the clarity of the filtrate. The floc has low viscosity and is not easy to block the filter screen. It improves the filtration speed and efficiency and achieves more efficient sludge dehydration.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer compound synthesis, and in particular to a cationic polymer suitable for chemical sludge dehydration and a preparation method thereof. Background Art
[0002] With the rapid development of industrialization and urbanization, the excessive sludge generated during sewage treatment is one of the challenges faced by sewage treatment plants. Sewage sludge not only has a high water content, is easy to rot, and has a strong odor, but also contains a large number of pathogenic bacteria, parasite eggs and other difficult-to-degrade heavy metals. If reasonable treatment and disposal methods are not adopted, it will cause irreversible damage to the ecological environment.
[0003] For chemical wastewater, the organic matter concentration is high and the chromaticity is high. It is often treated by combining physical and chemical methods with biological methods. The sludge produced is mainly chemical sludge and biological sludge. Chemical sludge has high organic matter content, relatively high calorific value and high recovery value, but the sludge has high viscosity and is difficult to dehydrate. Therefore, the harmlessness, reduction and resource utilization of chemical sludge are issues that urgently need to be addressed.
[0004] With the increasing attention paid to environmental issues, the requirements for chemical wastewater and sludge treatment are getting higher and higher, and chemical companies need to properly handle sludge. In the past, chemical companies used the traditional natural air drying method to dehydrate sludge. With the improvement of production efficiency and the expansion of production scale, the air drying method is obviously too backward. At present, most chemical companies use chemical flocculation and sedimentation followed by filter press dehydration. However, due to the high water content and high viscosity of the flocs after chemical flocculation, the filter cloth is easily blocked and damaged, and needs to be cleaned and replaced regularly. In addition, more operators are required, and the operation is somewhat complicated.
[0005] Huang Zhaoliang selected the printing and dyeing sludge (water content 97%) from a sewage treatment plant in Anqing City as the research object in "Research on the Influencing Factors and Optimization of Mechanical Filter Pressing Deep Dehydration of Printing and Dyeing Sludge" and used flocculants to modify the printing and dyeing sludge, deeply optimize the process, and reduce the moisture content of the mud cake to below 50%. Tian Ziyang pointed out the difficulty of sludge dehydration after flocculation by conventional flocculants in "Research Progress on the Application of Filter Aids in Sludge Dehydration", and pointed out that filter aids can form rigid and incompressible structures during the sludge dehydration process, construct filtrate channels, and improve sludge porosity and sludge dehydration efficiency. Huang Hua proposed in "Analysis of the Effect of Flocculants on Sludge Dehydration Efficiency and Calorific Value" that when the organic matter content in the sludge is ≤44% and the PAC agent addition rate is ≥2%, the plate and frame filter press is used for sludge filter pressing and dehydration, and the moisture content of the obtained mud cake basically meets ≤60%. However, the flocculants in the prior art still have the problems of high moisture content of filter cake after dehydration, low turbidity removal rate of filtrate and difficulty in dehydration during filter pressing in chemical sludge dehydration.
[0006] In summary, it is very necessary to research and develop a cationic polymer suitable for chemical sludge dehydration and a preparation method thereof. Summary of the invention
[0007] In order to solve one or more technical problems existing at present, such as high water content in chemical sludge dehydration, low turbidity removal rate of filtrate and difficulty in dehydration during filter pressing, the present invention provides a cationic polymer suitable for chemical sludge dehydration and a preparation method thereof.
[0008] In a first aspect, the present invention provides a method for preparing a cationic polymer suitable for dehydrating chemical sludge, the preparation method comprising the following steps:
[0009] (1) Allyl trimethyl ammonium chloride, N-methyl-N,N,N-triallylammonium chloride, dimethyl diallyl ammonium chloride and water are uniformly mixed to obtain a mixed system, and then the mixed system is nitrogen-free and oxygen-free, and then a chain transfer agent and an oxidant are added to react to obtain a destabilizing agent;
[0010] (2) adding chitosan to the acetic acid solution and mixing them evenly to obtain a chitosan solution, and then sequentially adding hexadecyltrimethylammonium chloride and a dialdehyde substance to the chitosan solution and stirring and ultrasonicating the mixture to obtain nano-chitosan;
[0011] (3) uniformly mixing acrylamide, cationic monomer, nano-chitosan, destabilizing agent, micro-crosslinking agent, dodecyl dimethyl benzyl ammonium chloride and water to obtain a mixed solution, and then adding a chain transfer agent, an azo initiator, an oxidant and a reducing agent to the mixed solution for reaction to obtain a polymer block;
[0012] (4) The polymer blocks are granulated, dried, ground and sieved in sequence to obtain a cationic polymer suitable for dehydration of chemical sludge.
[0013] Preferably, in step (1), the mass ratio of the allyltrimethylammonium chloride, N-methyl-N,N,N-triallylammonium chloride, dimethyldiallylammonium chloride and water is (70-90):(1-2):(15-20):100; the mass amount of the chain transfer agent is 0.1-0.3% of the sum of the mass amounts of the allyltrimethylammonium chloride, the N-methyl-N,N,N-triallylammonium chloride and the dimethyldiallylammonium chloride; and / or the mass amount of the oxidant is 0.3-0.5% of the sum of the mass amounts of the allyltrimethylammonium chloride, the N-methyl-N,N,N-triallylammonium chloride and the dimethyldiallylammonium chloride.
[0014] Preferably, in step (1): the chain transfer agent is sodium formate; and / or the oxidant is ammonium persulfate.
[0015] Preferably, in step (1): before nitrogen deoxygenation, the pH of the mixed system is adjusted to 4-5 and the temperature of the mixed system is adjusted to 45-50°C.
[0016] Preferably, the molecular weight of the destabilizing agent is 30,000 to 100,000.
[0017] Preferably, in step (2): the concentration of the acetic acid solution is 2-3wt%; the dosage ratio of the acetic acid solution, the chitosan, the hexadecyltrimethylammonium chloride and the dialdehyde substance is 100mL: (1.5-2.5)g: (0.5-1.5)g: (0.4-0.6)g; and / or the dialdehyde substance is glutaraldehyde and / or glyoxal.
[0018] Preferably, in step (3): the cationic monomer is triethyl (4-vinylbenzyl) ammonium chloride; the micro-crosslinking agent is tetraallyl ammonium chloride; the chain transfer agent is sodium hypophosphite; the azo initiator is azobisisobutylimidazoline hydrochloride; the oxidant is hydrogen peroxide; and / or the reducing agent is sodium bisulfite.
[0019] Preferably, in step (3): before nitrogen deoxygenation, the pH of the mixed solution is adjusted to 4-5 and the temperature of the mixed solution is adjusted to 15-18°C; and / or the raw materials used include, by weight, 20-40 parts of acrylamide, 250-350 parts of cationic monomer, 10-20 parts of nano-chitosan, 200-400 parts of destabilizing agent, 0.05-0.2 parts of micro-crosslinking agent, 2-8 parts of dodecyl dimethyl benzyl ammonium chloride, 132-508 parts of water, 0.01-0.02 parts of chain transfer agent, 0.05-0.1 parts of azo initiator, 0.005-0.01 parts of oxidant, and 0.005-0.01 parts of reducing agent.
[0020] Preferably, the molecular weight of the cationic polymer suitable for chemical sludge dehydration is 2 to 3 million.
[0021] In a second aspect, the present invention provides a cationic polymer suitable for dehydration of chemical sludge, which is prepared by the preparation method described in the first aspect of the present invention.
[0022] Compared with the prior art, the present invention has at least the following beneficial effects:
[0023] (1) The present invention polymerizes nano-chitosan, cationic monomers, acrylamide, and micro-crosslinking agents through a copolymerization process, and simultaneously introduces a destabilizing agent and a conditioning agent (dodecyl dimethyl benzyl ammonium chloride) into the prepared cationic polymer, so that the cationic polymer has a great electrical neutralization ability and sweeping ability during the dehydration of chemical sludge, and can make the suspended matter through electrical neutralization and bridging adsorption, and play a good flocculation effect.
[0024] (2) The destabilizing agent introduced into the cationic polymer of the present invention is a low molecular weight polymer with a high charge, which can quickly break the original equilibrium structure in the sludge and destabilize the sludge suspension. At the same time, the cationic polymer prepared by the present invention has a network structure and contains a large number of quaternary ammonium salt groups, which can combine with the ultrafine suspension in the sludge to quickly form small flocs. The network cationic polymer can further connect these small flocs to form a large number of dense flocs.
[0025] (3) The conditioning agent (dodecyl dimethyl benzyl ammonium chloride) and the destabilizing agent introduced in the present invention can also dissolve extracellular polymers and convert the water attached to the surface of the flocs into free water, which is beneficial to reduce the moisture content of the filter cake during the dehydration process.
[0026] (4) In the process of preparing the cationic polymer, the present invention forms a spatial network structure with nano-chitosan as the core through the grafting reaction of nano-chitosan with acrylamide and cationic monomers. At the same time, through the action of the micro-crosslinking agent, a micro-crosslinked network structure is formed between different molecular chains, which can significantly increase the sweeping area of the cationic polymer, make the flocs compact, and show better dehydration performance.
[0027] (5) The cationic polymer synthesized in the present invention is a low molecular weight polymer with good dehydration effect. After flocculation and dehydration, the viscosity of the flocs and the supernatant is low, the filtrate is clear, the flocs are compact, and it is not easy to clog the filter mesh. During compression dehydration, it helps to increase the filtration speed and can significantly reduce the moisture content of the filter cake. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0029] In a first aspect, the present invention provides a method for preparing a cationic polymer (abbreviated as cationic polymer) suitable for dehydration of chemical sludge, the preparation method comprising the following steps:
[0030] (1) Allyl trimethyl ammonium chloride, N-methyl-N,N,N-triallylammonium chloride, dimethyl diallyl ammonium chloride and water are uniformly mixed to obtain a mixed system, and then the mixed system is deoxygenated by nitrogen, and then a chain transfer agent and an oxidant are added to react (polymerization reaction) to obtain a destabilizing agent; in step (1) of the present invention, the reaction temperature is, for example, 45 to 50° C., and the reaction time is, for example, 3 to 5 hours;
[0031] (2) adding chitosan to the acetic acid solution and mixing evenly to obtain a chitosan solution, and then adding hexadecyltrimethylammonium chloride and a dialdehyde substance to the chitosan solution in sequence, stirring and ultrasonicating the solution to obtain nano-chitosan; the nano-chitosan in step (2) of the present invention can participate in the graft copolymerization reaction; in the present invention, using a dialdehyde substance as a cross-linking agent and using hexadecyltrimethylammonium chloride as a cationic surfactant can promote flocculation; the present invention has no special requirements for chitosan, and products that can be directly purchased on the market can be used. For example, the chitosan used can be chitosan with a molecular weight of 40kDa~70kDa; the present invention does not specifically limit the stirring and ultrasonicating conditions, and those skilled in the art can make conventional selections. The stirring speed can be, for example, 400~800r / min;
[0032] (3) acrylamide, cationic monomer, nano-chitosan, destabilizing agent, micro-crosslinking agent, dodecyl dimethyl benzyl ammonium chloride and water are uniformly mixed to obtain a mixed solution, and then the mixed solution is deoxygenated by nitrogen, and then a chain transfer agent, an azo initiator, an oxidant and a reductant are added to react (copolymerization reaction) to obtain a polymer block; in the present invention, dodecyl dimethyl benzyl ammonium chloride is used as a conditioning agent, which has a high cationic charge and can break the equilibrium state of ions in the original chemical wastewater, and also helps to destabilize the particles and cause collision flocculation; in step (3) of the present invention, for example, after the reaction is initiated at 15-18°C, the temperature of the reaction system will naturally rise, and after naturally rising to the peak temperature, continue to react at the peak temperature for 2-4 hours; in the present invention, unless otherwise specified, the various substances used can be products that can be directly purchased on the market or synthesized by existing methods;
[0033] (4) The polymer blocks are sequentially granulated, dried, ground and sieved to obtain a cationic polymer suitable for dehydrating chemical sludge. The present invention does not specifically limit the conditions for granulating, drying, grinding and sieving, and conventional conditions can be used.
[0034] The present invention polymerizes nano-chitosan, cationic monomers, acrylamide and micro-crosslinking agents through a copolymerization process, and at the same time introduces a destabilizing agent and a conditioning agent (dodecyl dimethyl benzyl ammonium chloride) into the prepared cationic polymer, so that the cationic polymer has great electrical neutralization and sweeping capabilities during chemical sludge dehydration, and can make suspended matter play a good flocculation effect through electrical neutralization and bridging adsorption. The destabilizing agent introduced into the cationic polymer of the present invention is a low-molecular-weight polymer with high charge, which can quickly break the original equilibrium structure in the sludge and destabilize the sludge suspended matter. At the same time, the cationic polymer prepared by the present invention has a network structure, contains a large number of quaternary ammonium salt groups, can combine with ultrafine suspended matter in the sludge, and quickly form small flocs. The network cationic polymer can further connect these small flocs to form a large number of dense flocs. The conditioning agent introduced into the present invention The agent (dodecyl dimethyl benzyl ammonium chloride) and the destabilizing agent can also dissolve extracellular polymers, and can convert the surface attached water of the flocs into free water, which is beneficial to reducing the moisture content of the filter cake during the dehydration process; in the process of preparing the cationic polymer, the present invention forms a spatial network structure with nano-chitosan as the core through the grafting reaction of nano-chitosan with acrylamide and cationic monomers. At the same time, through the action of the micro-crosslinking agent, a micro-crosslinking network structure is formed between different molecular chains, which can significantly increase the sweeping area of the cationic polymer, make the flocs compact, and show better dehydration performance; the cationic polymer synthesized by the present invention is a low molecular weight polymer with good dehydration effect. After flocculation and dehydration, the viscosity of the flocs and the supernatant can be low, the filtrate is clear, the flocs are compact, and it is not easy to clog the filter mesh. During compression dehydration, it is helpful to improve the filtration speed and greatly reduce the moisture content of the filter cake.
[0035] According to some preferred embodiments, in step (1), the mass ratio of allyltrimethylammonium chloride, N-methyl-N,N,N-triallylammonium chloride, dimethyldiallylammonium chloride and water is (70-90):(1-2):(15-20):100, more preferably 81:1:18:100. The destabilizing agent formed in this way has a high charge density and an appropriate molecular weight, which can quickly destabilize the particles to form small flocs, and enable the cationic polymer to play a better flocculation role. The mass amount of the chain transfer agent is 0.1-0.3% of the sum of the mass amounts of the allyltrimethylammonium chloride, the N-methyl-N,N,N-tripropylene ammonium chloride and the dimethyldiallylammonium chloride, preferably 0.2%; and / or the mass amount of the oxidant is 0.3-0.5% of the sum of the mass amounts of the allyltrimethylammonium chloride, the N-methyl-N,N,N-tripropylene ammonium chloride and the dimethyldiallylammonium chloride, preferably 0.4%.
[0036] According to some preferred embodiments, in step (1): the chain transfer agent is sodium formate; and / or the oxidant is ammonium persulfate.
[0037] According to some preferred embodiments, in step (1): before nitrogen deoxygenation, the pH of the mixed system is adjusted to 4-5 and the temperature of the mixed system is adjusted to 45-50°C.
[0038] According to some preferred embodiments, the molecular weight of the destabilizing agent is 30,000 to 100,000. The present invention finds that the destabilizing agent with a molecular weight in the range of 30,000 to 100,000 can not only quickly destabilize the particles, but also quickly undergo flocculation reaction to form small flocs. If the molecular weight of the destabilizing agent is too high, the reaction time is too slow, and the destabilization effect of the particles is poor. If the molecular weight of the destabilizing agent is too low, the flocculation effect of the cationic polymer will deteriorate, which is not conducive to the formation of small flocs.
[0039] According to some specific embodiments, the destabilizing agent is prepared using the following raw materials: allyltrimethylammonium chloride, N-methyl-N,N,N-tripropyleneammonium chloride, dimethyldiallylammonium chloride, water and acetic acid; the preparation method is: add allyltrimethylammonium chloride, N-methyl-N,N,N-tripropyleneammonium chloride, dimethyldiallylammonium chloride and water into a reactor, mix them thoroughly and evenly to obtain a mixed system, then add acetic acid to the mixed system to adjust the pH of the mixed system to 4~5 and adjust the temperature of the mixed system to 45~50°C, blow nitrogen to deoxygenate for 30 minutes, add a chain transfer agent and an oxidant to initiate a polymerization reaction to obtain the destabilizing agent; the present invention does not specifically limit the amount of acetic acid used to adjust the pH of the mixed system, as long as the pH of the mixed system can be adjusted to the target range.
[0040] According to some preferred embodiments, in step (2): the concentration of the acetic acid solution is 2-3wt%. In the present invention, the acetic acid solution is an acetic acid aqueous solution. The concentration of the acetic acid solution is 2-3wt%, which means that the mass fraction of acetic acid contained in the acetic acid aqueous solution is 2-3wt%; and / or the amount ratio of the acetic acid solution, the chitosan, the hexadecyltrimethylammonium chloride and the dialdehyde substance is 100mL: (1.5-2.5)g: (0.5-1.5)g: (0.4-0.6)g, preferably 100mL: 2g: 1g: 0.5g.
[0041] According to some preferred embodiments, in step (2): the dialdehyde substance is glutaraldehyde and / or glyoxal.
[0042] According to some specific embodiments, the preparation of the nano-chitosan uses the following raw materials: chitosan, acetic acid, hexadecyltrimethylammonium chloride, glutaraldehyde and water; the preparation method is: acetic acid is prepared into 100 mL of acetic acid solution with a concentration of 2.5wt% with water, 2g of chitosan is added, and stirred for 20min to make the chitosan completely dissolved, then 1g of hexadecyltrimethylammonium chloride is added, and after stirring evenly, 0.5g of glutaraldehyde is added, and after stirring evenly, ultrasonication is performed for 5min to obtain nano-chitosan.
[0043] According to some preferred embodiments, in step (3): the cationic monomer is triethyl (4-vinylbenzyl) ammonium chloride (also known as N-triethyl-(4-vinylbenzyl) ammonium chloride); the micro-crosslinking agent is tetraallyl ammonium chloride; the chain transfer agent is sodium hypophosphite; the azo initiator is azobisisobutylimidazoline hydrochloride; the oxidant is hydrogen peroxide; and / or the reducing agent is sodium bisulfite.
[0044] According to some preferred embodiments, in step (3): before nitrogen deoxygenation, the pH of the mixed solution is adjusted to 4-5 and the temperature of the mixed solution is adjusted to 15-18°C; and / or the raw materials used include 20-40 parts (e.g., 20, 25, 30, 35 or 40 parts) of acrylamide, 250-350 parts (e.g., 250, 260, 270, 280, 290, 300, 310, 320, 330, 340 or 350 parts) of cationic monomer by weight. , nano chitosan 10-20 parts (e.g. 10, 11, 12, 131, 415, 16, 17, 18, 19 or 20 parts), destabilizing agent 200-400 parts (e.g. 200, 250, 300, 350 or 400 parts), micro cross-linking agent 0.05-0.2 parts (e.g. 0.05, 0.1, 0.15 or 0.2 parts), dodecyl dimethyl benzyl ammonium chloride 2-8 parts (e.g. 2, 3, 4, 5, 6, 7 or 8 parts), water 132-508 parts (e.g. 132, 150, 180, 200, 250, 300, 350, 400, 450, 500 or 508 parts), chain transfer agent 0.01-0.02 parts (for example, 0.01, 0.015 or 0.02 parts), azo initiator 0.05-0.1 parts (for example, 0.05, 0.06, 0.07, 0.08, 0.09 or 0.1 parts), oxidant 0.005-0.01 parts (for example, 0.005, 0.008 or 0.01 parts), reducing agent 0.005-0.01 parts (for example, 0 .005, 0.008 or 0.01 parts); in the present invention, preferably, the mass ratio of the acrylamide, cationic monomer, nano-chitosan and destabilizing agent is (20-40): (250-350): (10-20): (200-400), which is more conducive to obtaining the cationic polymer suitable for chemical sludge dehydration, which can make the dehydration performance better and the filtrate turbidity lower during chemical sludge dehydration, and can help to improve the filtration speed and make the filter cake water content lower during compression dehydration.
[0045] In the present invention, "parts" refer to "parts by weight". In specific embodiments and comparative examples, the units of parts by weight can be unified into weight units such as "g" or "kg". In the present invention, "and / or" between multiple technical features indicates that these technical features are connected in an "and / or" relationship, indicating that it can be any one of these technical features, or a combination of any two or more of these technical features.
[0046] According to some preferred embodiments, the molecular weight of the prepared cationic polymer suitable for dehydration of chemical sludge is 2 to 3 million; in the present invention, preferably, the molecular weight of the cationic polymer suitable for dehydration of chemical sludge is 2 to 3 million, the cationic polymer has a low molecular weight, a short reaction time with the particles, can quickly form flocs, the formed flocs are relatively small, and there is less water wrapped between the flocs, which is conducive to dehydration, and the cationic polymer has a low molecular weight, and the sewage viscosity is low after addition, which is conducive to floc sedimentation; in the present invention, the molecular weights of the destabilizing agent and the cationic polymer are measured according to the test method 5.2 in the standard GB / T 31246-2014.
[0047] According to some specific embodiments, the preparation of the cationic polymer suitable for chemical sludge dehydration adopts the following raw materials in parts by weight: 20-40 parts of acrylamide, 250-350 parts of cationic monomers, 10-20 parts of nano-chitosan, 200-400 parts of destabilizing agents, 0.05-0.2 parts of micro-crosslinking agents, 2-8 parts of conditioning agents (dodecyl dimethyl benzyl ammonium chloride), 132-508 parts of water, 0.01-0.02 parts of chain transfer agents, 0.05-0.1 parts of azo initiators, 0.005-0.01 parts of oxidants, and 0.005-0.01 parts of reducing agents; the preparation method is: acrylamide, cationic monomers, nano-chitosan, 200-400 parts of destabilizing agents, 0.05-0.2 parts of micro-crosslinking agents, 2-8 parts of conditioning agents (dodecyl dimethyl benzyl ammonium chloride), 132-508 parts of water, 0.01-0.02 parts of chain transfer agents, 0.05-0.1 parts of azo initiators, 0.005-0.01 parts of oxidants, and 0.005-0.01 parts of reducing agents. Polysaccharide, a destabilizing agent, a micro-crosslinking agent, dodecyldimethylbenzyl ammonium chloride and water are uniformly mixed to obtain a mixed solution; after adjusting the pH value of the mixed solution to 4-5 with acetic acid and adjusting the temperature of the mixed solution to 15-18°C, nitrogen is blown for deoxygenation for 30 minutes, a chain transfer agent, an azo initiator, an oxidant and a reductant are added to initiate a copolymerization reaction to obtain a polymer block; the polymer block is granulated, dried, ground and sieved to obtain a cationic polymer (abbreviated as a cationic polymer) suitable for chemical sludge dehydration; the present invention does not specifically limit the amount of acetic acid used for adjusting the pH value of the mixed solution, and the pH value of the mixed solution can be adjusted to a target range.
[0048] In a second aspect, the present invention provides a cationic polymer suitable for dehydration of chemical sludge, which is prepared by the preparation method described in the first aspect of the present invention.
[0049] The present invention will be further described below by way of examples, but the protection scope of the present invention is not limited to these embodiments.
[0050] In the present invention, the preparation of destabilizing agent A is:
[0051] Add 81 parts of allyltrimethylammonium chloride, 1 part of N-methyl-N,N,N-triallylammonium chloride, 18 parts of dimethyldiallylammonium chloride and 100 parts of water into a reactor, mix them thoroughly to obtain a mixed system, then add acetic acid to the mixed system and adjust the pH of the mixed system to 4.5, and adjust the temperature of the mixed system to 47°C, blow nitrogen to deoxygenate for 30 minutes, then add 0.2 parts of sodium formate and 0.4 parts of ammonium persulfate and react at 47°C. After reacting for 4 hours, a destabilizer A with a molecular weight of 46,000 is obtained.
[0052] In the present invention, the preparation of destabilizing agent B is:
[0053] Add 50 parts of allyltrimethylammonium chloride, 50 parts of dimethyldiallylammonium chloride and 100 parts of water into a reactor, mix them thoroughly to obtain a mixed system, then add acetic acid to the mixed system and adjust the pH of the mixed system to 4.5, and adjust the temperature of the mixed system to 47°C, blow nitrogen to deoxygenate for 30 minutes, then add 0.2 parts of sodium formate and 0.4 parts of ammonium persulfate, react at 47°C, and react for 4 hours to obtain a destabilizing agent B.
[0054] In the present invention, the preparation of the destabilizing agent C is:
[0055] Add 50 parts of allyltrimethylammonium chloride, 10 parts of N-methyl-N,N,N-triallylammonium chloride, 40 parts of dimethyldiallylammonium chloride and 100 parts of water into a reaction kettle, mix them thoroughly to obtain a mixed system, then add acetic acid to the mixed system and adjust the pH of the mixed system to 4.5, and adjust the temperature of the mixed system to 47°C, blow nitrogen to deoxygenate for 30 minutes, add 0.2 parts of sodium formate and 0.4 parts of ammonium persulfate, react at 47°C, and react for 4 hours to obtain a destabilizing agent C.
[0056] In the present invention, the preparation of the destabilizing agent D is:
[0057] Add 81 parts of allyltrimethylammonium chloride, 1 part of N-methyl-N,N,N-triallylammonium chloride, 18 parts of dimethyldiallylammonium chloride and 100 parts of water into a reactor, mix them thoroughly to obtain a mixed system, then add acetic acid to the mixed system and adjust the pH of the mixed system to 4.5, and adjust the temperature of the mixed system to 47°C, blow nitrogen to deoxygenate for 30 minutes, then add 1 part of sodium formate and 0.4 parts of ammonium persulfate and react at 47°C. After reacting for 4 hours, a destabilizer D with a molecular weight of 8,000 is obtained.
[0058] In the following examples and comparative examples, the preparation of the nano-chitosan used is:
[0059] Acetic acid is prepared into an acetic acid solution with a concentration of 2.5wt% by water, and then chitosan is added and stirred for 20 minutes to make the chitosan completely dissolved, and then hexadecyltrimethylammonium chloride is added, and after stirring and mixing evenly, glutaraldehyde is added, and after stirring and mixing evenly, ultrasonication is performed for 5 minutes to obtain nano chitosan; wherein the amount ratio of the acetic acid solution, the chitosan, the hexadecyltrimethylammonium chloride and the glutaraldehyde is 100mL:2g:1g:0.5g.
[0060] Example 1
[0061] The present embodiment provides a method for preparing a cationic polymer suitable for dehydrating chemical sludge; the raw materials used in the preparation of the cationic polymer suitable for dehydrating chemical sludge are: 20 parts of acrylamide, 250 parts of triethyl (4-vinyl benzyl) ammonium chloride, 10 parts of nano-chitosan, 200 parts of destabilizing agent A, 0.05 parts of tetraallyl ammonium chloride, 2 parts of dodecyl dimethyl benzyl ammonium chloride, 508 parts of water, 0.01 parts of sodium hypophosphite, 0.05 parts of azobisisobutylimidazoline hydrochloride, 0.005 parts of hydrogen peroxide and 0.005 parts of sodium bisulfite; the preparation method is: acrylamide, triethyl (4-vinyl benzyl) ammonium chloride, nano-chitosan, destabilizing agent A, tetraallyl ammonium chloride, dodecyl dimethyl benzyl ammonium chloride and water are uniformly mixed to obtain a mixed solution, and acetic acid is used to adjust the mixture. The pH value of the mixed solution was set to 4, and the temperature of the mixed solution was adjusted to 15°C. Nitrogen was blown for deoxygenation for 30 minutes. Sodium hypophosphite, azobis(isobutylene)imidazoline hydrochloride, hydrogen peroxide and sodium bisulfite were added to react. The reaction system was naturally heated to the peak temperature and reacted at the peak temperature for 3 hours to complete the reaction, thereby obtaining polymer lumps. The polymer lumps were granulated, dried, ground and sieved to obtain a cationic polymer (abbreviated as cationic polymer) with a molecular weight of 2.85 million suitable for chemical sludge dehydration.
[0062] Example 2
[0063] The present embodiment provides a method for preparing a cationic polymer suitable for dehydrating chemical sludge; the raw materials used in the preparation of the cationic polymer suitable for dehydrating chemical sludge are: 30 parts of acrylamide, 300 parts of triethyl (4-vinyl benzyl) ammonium chloride, 15 parts of nano-chitosan, 300 parts of destabilizing agent A, 0.1 parts of tetraallyl ammonium chloride, 5 parts of dodecyl dimethyl benzyl ammonium chloride, 350 parts of water, 0.015 parts of sodium hypophosphite, 0.07 parts of azobisisobutylimidazoline hydrochloride, 0.008 parts of hydrogen peroxide and 0.008 parts of sodium bisulfite; the preparation method is: acrylamide, triethyl (4-vinyl benzyl) ammonium chloride, nano-chitosan, destabilizing agent A, tetraallyl ammonium chloride, dodecyl dimethyl benzyl ammonium chloride and water are uniformly mixed to obtain a mixed solution, and the mixed solution is adjusted with acetic acid. The pH value of the mixed solution is 4.5, and after adjusting the temperature of the mixed solution to 17°C, nitrogen is blown for deoxygenation for 30 minutes, and sodium hypophosphite, azobisisobutylimidazoline hydrochloride, hydrogen peroxide and sodium bisulfite are added to react. The reaction system is naturally heated to the peak temperature and reacts at the peak temperature for 2.5 hours to complete the reaction, thereby obtaining a polymer block. The polymer block is granulated, dried, ground and sieved to obtain a cationic polymer (abbreviated as a cationic polymer) with a molecular weight of 2.53 million suitable for chemical sludge dehydration.
[0064] Example 3
[0065] The present embodiment provides a method for preparing a cationic polymer suitable for dehydrating chemical sludge; the raw materials used in the preparation of the cationic polymer suitable for dehydrating chemical sludge are: 40 parts of acrylamide, 350 parts of triethyl (4-vinyl benzyl) ammonium chloride, 20 parts of nano-chitosan, 400 parts of destabilizing agent A, 0.2 parts of tetraallyl ammonium chloride, 8 parts of dodecyl dimethyl benzyl ammonium chloride, 132 parts of water, 0.02 parts of sodium hypophosphite, 0.1 parts of azobisisobutylimidazoline hydrochloride, 0.01 parts of hydrogen peroxide and 0.01 parts of sodium bisulfite; the preparation method is: acrylamide, triethyl (4-vinyl benzyl) ammonium chloride, nano-chitosan, destabilizing agent A, tetraallyl ammonium chloride, dodecyl dimethyl benzyl ammonium chloride and water are uniformly mixed to obtain a mixed solution, and the mixed solution is adjusted with acetic acid. The pH value of the liquid is 5, and the temperature of the mixed liquid is adjusted to 18°C. Nitrogen is blown for deoxygenation for 30 minutes. Sodium hypophosphite, azobis(isobutylimidazoline) hydrochloride, hydrogen peroxide and sodium bisulfite are added to react. The reaction system is naturally heated to the peak temperature and reacts at the peak temperature for 2.5 hours to complete the reaction, thereby obtaining a polymer block. The polymer block is granulated, dried, ground and sieved to obtain a cationic polymer (abbreviated as a cationic polymer) with a molecular weight of 2.27 million suitable for chemical sludge dehydration.
[0066] Example 4
[0067] Embodiment 4 is substantially the same as Embodiment 1, except that:
[0068] In the preparation of cationic polymers, destabilizing agent B was used instead of destabilizing agent A for experiments.
[0069] Example 5
[0070] Example 5 is substantially the same as Example 1, except that:
[0071] In the preparation of cationic polymers, destabilizing agent C was used instead of destabilizing agent A for experiments.
[0072] Example 6
[0073] Embodiment 6 is substantially the same as Embodiment 1, except that:
[0074] In the preparation of cationic polymers, destabilizing agent D was used instead of destabilizing agent A for experiments.
[0075] Comparative Example 1
[0076] Comparative Example 1 is substantially the same as Example 1, except that:
[0077] The raw materials for preparing the cationic polymer do not contain the destabilizing agent A, and the destabilizing agent A is not added during the process of preparing the cationic polymer.
[0078] Comparative Example 2
[0079] Comparative Example 2 is substantially the same as Example 1, except that:
[0080] The raw materials for preparing the cationic polymer do not contain nano-chitosan, and no nano-chitosan is added during the process of preparing the cationic polymer.
[0081] Comparative Example 3
[0082] Comparative Example 3 is substantially the same as Example 1, except that:
[0083] The amount of triethyl (4-vinylbenzyl) ammonium chloride added was 20 parts, and the amount of acrylamide added was 250 parts.
[0084] Comparative Example 4
[0085] Comparative Example 4 is substantially the same as Example 1, except that:
[0086] The raw materials for preparing the cationic polymer do not contain dodecyldimethylbenzylammonium chloride, and dodecyldimethylbenzylammonium chloride is not added during the process of preparing the cationic polymer.
[0087] Comparative Example 5
[0088] Comparative Example 5 is substantially the same as Example 1, except that:
[0089] The raw materials for preparing the cationic polymer do not contain tetraallyl ammonium chloride, and no tetraallyl ammonium chloride is added during the preparation of the cationic polymer.
[0090] Comparative Example 6
[0091] Comparative Example 6 is substantially the same as Example 1, except that:
[0092] The raw materials for preparing the cationic polymer do not contain sodium hypophosphite, and no sodium hypophosphite is added during the process of preparing the cationic polymer.
[0093] The cationic polymer obtained in this comparative example has very poor solubility and cannot be tested for performance.
[0094] Comparative Example 7
[0095] Comparative Example 7 is substantially the same as Example 1, except that:
[0096] In the preparation of cationic polymers, chitosan was used instead of nano-chitosan for experiments.
[0097] Comparative Example 8
[0098] The present comparative example provides a method for preparing a cationic polymer; the raw materials used in the preparation of the cationic polymer are: 20 parts of acrylamide, 250 parts of triethyl (4-vinyl benzyl) ammonium chloride, 10 parts of nano-chitosan, 200 parts of polydimethyldiallylammonium chloride (molecular weight 50,000, content 50wt%), 0.05 parts of tetraallylammonium chloride, 2 parts of dodecyldimethylbenzyl ammonium chloride, 508 parts of water, 0.01 parts of sodium hypophosphite, 0.05 parts of azobisisobutylimidazoline hydrochloride, 0.005 parts of hydrogen peroxide and 0.005 parts of sodium bisulfite; the preparation method is: acrylamide, triethyl (4-vinyl benzyl) ammonium chloride, 10 parts of nano-chitosan, 200 parts of polydimethyldiallylammonium chloride (molecular weight 50,000, content 50wt%), 0.05 parts of tetraallylammonium chloride, 2 parts of dodecyldimethylbenzyl ammonium chloride, 508 parts of water, 0.01 parts of sodium hypophosphite, 0.05 parts of azobisisobutylimidazoline hydrochloride, 0.005 parts of hydrogen peroxide and 0.005 parts of sodium bisulfite; The mixture is uniformly mixed with (4-vinylbenzyl) ammonium chloride, nano-chitosan, polydimethyldiallylammonium chloride, tetraallylammonium chloride, dodecyldimethylbenzyl ammonium chloride and water to obtain a mixed solution, the pH value of the mixed solution is adjusted to 4 with acetic acid, and the temperature of the mixed solution is adjusted to 15°C, and then nitrogen is blown for deoxygenation for 30 minutes, and sodium hypophosphite, azobisisobutylimidazoline hydrochloride, hydrogen peroxide and sodium bisulfite are added to react, the reaction system is naturally heated to a peak temperature and reacted at the peak temperature for 3 hours to complete the reaction, and a polymer block is obtained, and the polymer block is granulated, dried, ground and sieved to obtain a cationic polymer.
[0099] The present invention conducts comparative performance evaluation on the cationic polymers prepared in various embodiments and comparative examples.
[0100] Test sample: The test sample was taken from the sludge water sample of a chemical company in Dongying City, Shandong Province.
[0101] Test method: Take 99mL of chemical sludge water sample, pour it into a measuring cylinder, add 1mL of 1000ppm cationic polymer aqueous solution, close the measuring cylinder mouth, shake it up and down three times, record the time from 100mL to 60mL as the sedimentation time, record the height of the flocs after sedimentation for 10min as the compressed volume, and analyze the turbidity removal rate of the supernatant with a turbidity meter. Use an experimental micro plate-frame filter press to simulate the effect of plate-frame filtration after flocculation of cationic polymers in different embodiments and different comparative examples, and test the moisture content of filter cakes of different cationic polymers after flocculation and filtration. The results are shown in Table 1 below.
[0102] Table 1
[0103]
[0104] It can be seen from the experimental data in Table 1 that the cationic polymer prepared by the method of the present invention can destabilize the suspended particles of sewage through the destabilizing agent, and form compact small flocs with organic matter in chemical sludge, and the cationic polymer can connect the flocs together through charge neutralization, adsorption bridging and sweeping action. The flocs have strong rigidity, low viscosity and weak viscosity. At the same time, under the joint action of the conditioning agent (dodecyldimethylbenzylammonium chloride) and the destabilizing agent, part of the adsorbed water on the surface of the flocs can be converted into free water, further reducing the moisture content of the filter cake; when the cationic polymer in some preferred embodiments of the present invention is used for dehydrating chemical sludge, the sedimentation time can be controlled within 5s, the compression volume can be controlled within 25mL, the turbidity removal rate is above 95%, and the moisture content of the filter cake can be controlled within 35-40%.
[0105] Parts of the present invention that are not described in detail are well known to those skilled in the art.
[0106] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a cationic polymer suitable for dehydration of chemical sludge, characterized in that: The preparation method comprises the following steps: (1) Allyl trimethyl ammonium chloride, N-methyl-N,N,N-triallylammonium chloride, dimethyl diallyl ammonium chloride and water are uniformly mixed to obtain a mixed system, and then the mixed system is deoxygenated by nitrogen, and then a chain transfer agent and an oxidant are added to react to obtain a destabilizing agent; the molecular weight of the destabilizing agent is 30,000 to 100,000; in step (1): the chain transfer agent is sodium formate, and the oxidant is ammonium persulfate; the mass ratio of allyl trimethyl ammonium chloride, N-methyl-N,N,N-triallylammonium chloride, dimethyl diallyl ammonium chloride and water is (70-90): (1-2): (15-20): 100; the mass amount of the chain transfer agent is 0.1-0.3% of the sum of the mass amounts of the allyl trimethyl ammonium chloride, the N-methyl-N,N,N-triallylammonium chloride and the dimethyl diallyl ammonium chloride; (2) adding chitosan to the acetic acid solution and mixing them evenly to obtain a chitosan solution, and then sequentially adding hexadecyltrimethylammonium chloride and a dialdehyde substance to the chitosan solution and stirring and ultrasonicating the mixture to obtain nano-chitosan; (3) In parts by weight, 20-40 parts of acrylamide, 250-350 parts of cationic monomer, 10-20 parts of nano-chitosan, 200-400 parts of destabilizing agent, 0.05-0.2 parts of micro-crosslinking agent, 2-8 parts of dodecyl dimethyl benzyl ammonium chloride and 132-508 parts of water are mixed evenly to obtain a mixed solution, and then the mixed solution is deoxygenated by nitrogen, and then 0.01-0.02 parts of chain transfer agent, 0.05-0.1 parts of azo initiator, 0.005-0.01 parts of oxidant and 0.005-0.01 parts of reducing agent are added to react to obtain a polymer block; in step (3), the cationic monomer is triethyl (4-vinyl benzyl) ammonium chloride, the micro-crosslinking agent is tetraallyl ammonium chloride, the chain transfer agent is sodium hypophosphite, the oxidant is hydrogen peroxide, and the reducing agent is sodium bisulfite; (4) The polymer blocks are granulated, dried, ground and sieved in sequence to obtain a cationic polymer suitable for dehydration of chemical sludge.
2. The preparation method according to claim 1, characterized in that: In step (1): The mass dosage of the oxidant is 0.3-0.5% of the sum of the mass dosages of the allyltrimethylammonium chloride, the N-methyl-N,N,N-triallylammonium chloride and the dimethyldiallylammonium chloride.
3. The preparation method according to claim 1, characterized in that: In step (1): Before nitrogen deoxygenation, the pH of the mixed system is adjusted to 4-5 and the temperature of the mixed system is adjusted to 45-50°C.
4. The preparation method according to claim 1, characterized in that: In step (2): The concentration of the acetic acid solution is 2-3wt%; The usage ratio of the acetic acid solution, the chitosan, the hexadecyltrimethylammonium chloride and the dialdehyde substance is 100 mL: (1.5-2.5) g: (0.5-1.5) g: (0.4-0.6) g; And / or the dialdehyde substance is glutaraldehyde and / or glyoxal.
5. The preparation method according to claim 1, characterized in that: In step (3): The azo initiator is azobisisobutylimidazoline hydrochloride.
6. The preparation method according to claim 1, characterized in that: In step (3): Before nitrogen deoxygenation, the pH of the mixed solution is adjusted to 4-5 and the temperature of the mixed solution is adjusted to 15-18°C.
7. The preparation method according to claim 1, characterized in that: The molecular weight of the prepared cationic polymer suitable for chemical sludge dehydration is 2 to 3 million.
8. A cationic polymer suitable for dehydration of chemical sludge obtained by the preparation method according to any one of claims 1 to 7.
Citation Information
Patent Citations
Cationic polymer for sludge dewatering and preparation method thereof
CN116284565A
Manufacturing and applicaition methods of water dispersant which containing chitosan type cationic acrylamide copolymer