An offshore photovoltaic floating material made of recyclable HDPE

By using circulating HDPE and anti-fouling sustained release agents in offshore photovoltaic floating materials, the problem of chewing fish is solved, and the anti-bite and corrosion resistance of floating materials is achieved, which extends the service life and reduces environmental pollution. risk.

CN118620306BActive Publication Date: 2024-11-22JIANGSU ANTOP POLYMER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410754234.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-11-22
Estimated Expiration
2044-06-12

AI Technical Summary

Technical Problem

The existing offshore photovoltaic floating materials are easily bitten by marine fish, resulting in a reduced service life and the gnawed floating materials are difficult to digest, causing environmental pollution and life safety threats.

Method used

Floating materials made of recyclable high-density polyethylene (HDPE) are used to improve the anti-adhesion performance of the floating body by adding anti-fouling sustained release agents, and eliminate fish through the sustained release effect of mothballs. , achieve anti-bite effect.

Benefits of technology

It significantly improves the anti-bite performance and corrosion resistance of floating materials, avoids the attachment of marine microorganisms and algae, reduces the risk of fish bites, and extends the service life of floating bodies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004888985000000101
    Figure BDA0004888985000000101
  • Figure BDA0004888985000000111
    Figure BDA0004888985000000111
Patent Text Reader

Abstract

The present invention relates to an offshore photovoltaic floating material made of recyclable HDPE, belonging to the technical field of floating material preparation. The floating material comprises the following raw materials by weight: 100 parts of HDPE and 10-25 parts of antifouling slow-release agent; the antifouling slow-release agent comprises 20-30 parts of dispersion, 10-20 parts of carrier and 30-40 parts of mothball powder. The dispersion is a hyperbranched polymer containing capsaicin structure and siloxane chain. The present invention, through the introduction of antifouling slow-release agent, improves the anti-attachment performance of the floating body on the one hand, avoids algae and fungi in the ocean from parasitizing on the floating body, and thus avoids tempting petrel fish to bite the floating body; on the other hand, it can slowly release mothballs, and utilize the effect of mothballs to expel fish, so that fish are unwilling to approach the floating body, thereby avoiding the biting of the floating body by fish.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparation of floating materials applied to offshore photovoltaics, and in particular, relates to a floating material made of recyclable HDPE. Background Art

[0002] High-density polyethylene (HDPE) is a type of polyethylene with good wear resistance, electrical insulation, toughness, cold resistance, and chemical stability. At room temperature, it is insoluble in any organic solvent, resistant to corrosion by acids, alkalis, and various salts, and has low water absorption. Therefore, HDPE is often used as a floating material on the water surface, such as the floating body used in offshore photovoltaics.

[0003] However, existing floating materials for offshore photovoltaics are often threatened by the gnawing of marine fish, which means that offshore floating bodies made of HDPE need to be replaced frequently, reducing their service life. In addition, HDPE eaten by fish is difficult to digest and accumulates along the food chain, eventually endangering human life safety.

[0004] Based on this, the present invention provides an offshore photovoltaic floating material made of recyclable HDPE. Summary of the invention

[0005] The purpose of the present invention is to provide an offshore photovoltaic floating body material made of recyclable HDPE, by adding an antifouling slow-release agent to the recyclable HDPE base material to solve the problem that the offshore floating body is easily bitten by marine fish, achieve the effect of inherently expelling marine fish, and realize the purpose of preventing the offshore floating body from being bitten.

[0006] The reasons why marine fish bite floating objects can be attributed to the following: First, the floating objects provide an attachment matrix for marine microorganisms or algae on the ocean surface. The marine microorganisms or algae attached and grown on the surface of the floating objects are undoubtedly very attractive to marine fish, thus tempting petrels to bite the floating objects; second, marine fish themselves bite the floating objects because of hunger, and the plastic particles on the floating objects are soaked into the stomach and intestines of marine fish and are difficult to digest, making the marine fish feel full, and thus making food-deficient marine organisms like to bite the floating objects.

[0007] Therefore, based on the above reasons why marine fish bite the floating body, the present invention needs to consider two issues to solve the technical problem: one is the problem of the attachment of marine microorganisms or algae on the floating body; the other is the likes and dislikes of marine fish for the floating body materials that have been gnawed.

[0008] The purpose of the present invention can be achieved by the following technical solutions:

[0009] An offshore photovoltaic floating material made of recyclable HDPE, comprising the following raw materials in parts by weight:

[0010] 100 parts of HDPE and 10-25 parts of antifouling slow-release agent.

[0011] Furthermore, the antifouling slow-release agent comprises 20-30 parts of dispersion, 10-20 parts of carrier and 30-40 parts of mothball powder.

[0012] Furthermore, the dispersion is a hyperbranched polymer formed by the stepwise reaction of N-hydroxymethyl acrylamide, 3,5-dimethylanisole, pentaerythritol, epoxysilane coupling agent and dimethylchlorosilane, and its molecular structure contains capsaicin structure and siloxane chain, and is specifically prepared by the following steps:

[0013] A1, after ethanol, N-hydroxymethyl acrylamide and 3,5-dimethyl anisole are uniformly mixed, sulfuric acid is slowly added dropwise, and after the addition is complete, the temperature is heated to 30-35°C, and the reaction is monitored by TLC plate. After the reaction is completed, a large amount of white crystal precipitates are precipitated after water is added, filtered, washed with deionized water until the filtrate is neutral, dried to obtain a crude product, and recrystallized with ethanol to obtain A2 type monomer, wherein the mass fraction of the sulfuric acid is 98%, the molar ratio of the N-hydroxymethyl acrylamide and the 3,5-dimethyl anisole is 2.4-3:1, and the mass of H2SO4 in the sulfuric acid is 0.1-5% of the total mass of N-hydroxymethyl acrylamide and 3,5-dimethyl anisole;

[0014] The A2-type monomer molecular structure contains a double-terminal double bond (derived from N-hydroxymethyl acrylamide);

[0015] A2. After pentaerythritol and tetrahydrofuran are uniformly mixed, the pH value of the mixed solution is adjusted to 10-11, the temperature is raised to 50-60° C., and the epoxy silane coupling agent is slowly added dropwise under stirring. After the addition is complete, the reaction is continued for 2-3 hours, the reaction is stopped, the mixture is rotary evaporated, washed with water, and vacuum dried to obtain a pentaerythritol derivative, wherein the molar ratio of the pentaerythritol to the epoxy silane coupling agent is 1:1;

[0016] A3, after the pentaerythritol derivative and dimethyl sulfoxide are uniformly mixed, potassium carbonate and potassium iodide are added under stirring, the mixture is heated to 90-95°C, dimethylchlorosilane is slowly added dropwise, and after the addition is complete, the reaction is continued with stirring for 6-12 hours, the reaction is stopped, the temperature is lowered, vacuum rotary evaporation is performed, and vacuum drying is performed to obtain a B3 type monomer, wherein the molar ratio of the pentaerythritol derivative, potassium carbonate, and dimethylchlorosilane is 1:3-5:3.1-3.5, and the mass of potassium iodide added is 1-5% of the total mass of the pentaerythritol derivative and dimethylchlorosilane;

[0017] The molecular structure of the B3 type monomer contains three silicon-hydrogen bonds (derived from dimethylsilyl chloride), and the silicon-hydrogen bonds are introduced into the pentaerythritol derivative by utilizing the etherification reaction between the hydroxyl group in the pentaerythritol derivative and the chlorine in the dimethylsilyl chloride;

[0018] A4. After uniformly mixing the A2 monomer, the B3 monomer and toluene, heat to 90-95° C. under nitrogen protection, then add chloroplatinic acid isopropanol solution, stir and react at constant temperature for 10-16 hours, adsorb the platinum catalyst with activated carbon after the reaction, filter, and remove the solvent by rotary evaporation to obtain a dispersion, wherein the mass ratio of the A2 monomer to the B3 monomer is 10:18-25, the amount of chloroplatinic acid isopropanol solution added is 3-8% of the total mass of the A2 monomer and the B3 monomer, and the mass fraction of chloroplatinic acid in the chloroplatinic acid isopropanol solution is 1%.

[0019] In the reaction of the A2-type monomer and the B3-type monomer, by utilizing double bonds and hydrosilylation polymerization, it can be seen that the resulting dispersion is a hyperbranched polymer, and its molecular formula contains a capsaicin structure, a siloxane structure, and other characteristics of a hyperbranched polymer.

[0020] Furthermore, the carrier is a porous adsorption particle, such as a mixture of one or more of porous silica, porous carbon, porous carbon nanorods, and porous graphene in any ratio. Preferably, it is porous carbon.

[0021] Furthermore, the antifouling slow-release agent is prepared by the following steps:

[0022] The carrier and the mothball powder are stirred and mixed evenly, and then the dispersion is added and mixed evenly, and then transferred to an extruder, extruded and granulated to obtain an antifouling slow-release agent, wherein the extrusion temperature is 170-210°C.

[0023] Furthermore, the floating material also includes the following raw materials in parts by weight: 1-5 parts of anti-ultraviolet agent and 1-5 parts of antioxidant.

[0024] By introducing anti-ultraviolet agents and antioxidants, the anti-ultraviolet performance and anti-aging performance of the obtained floating material can be improved, and the service life of the obtained floating material in sea surface application can be further improved.

[0025] The anti-ultraviolet agent and the antioxidant are additives well known in the technical field, and the present invention will not elaborate on them here.

[0026] Beneficial effects of the present invention:

[0027] In order to fundamentally solve the problem of marine fish biting floating bodies, the present invention starts from the root cause. On the one hand, the antifouling slow-release agent is used to improve the anti-attachment performance of the floating body, so as to prevent algae and fungi in the ocean from parasitizing on the floating body, thereby avoiding the temptation of petrel fish to bite the floating body. The explanation is as follows: first, the antifouling slow-release agent contains a large amount of siloxane chains, and the low surface energy characteristics of the molecular chain are used to give the floating body material a fouling-resistant property. Second, the antifouling slow-release agent contains a large amount of capsaicin structure (derived from 3,5-dimethylanisole), which has the effect of inhibiting and repelling the attachment of algae and fungi to the floating body; the other In one aspect, the antifouling slow-release agent can release mothballs slowly, and the mothballs can be used to drive away fish, so that fish are unwilling to approach the floating body, thereby avoiding the biting of the floating body by fish. The explanation is that the antifouling slow-release agent is wrapped with slow-release mothballs, and in the present invention, the carrier mothballs of the porous adsorption particles are first loaded, and then the carrier is dispersed and wrapped by the dispersion of the hyperbranched polymer with siloxane, which improves the loading effect and slow-release effect of the mothballs (double slow-release, adsorption slow-release and wrapping slow-release) on the one hand, and on the other hand, siloxane avoids the problem of the difficulty of dispersing the porous adsorption particle carrier in the organic matrix;

[0028] Remarkably, the dispersion plays multiple roles in the present invention. First, it is a wrapping agent that wraps the carrier and the mothballs to improve the sustained-release effect of the mothballs. Second, it has a dispersing effect. Its hyperbranched structure, on the one hand, makes the obtained antifouling sustained-release agent dispersed evenly in the HDPE, and on the other hand, makes the mothballs carried by the carrier evenly wrapped by the dispersion. Third, its siloxane structure and capsaicin structure play an antifouling and anti-adhesion role, repel fungi and microorganisms, and improve the corrosion resistance (siloxane chain effect) and rigidity (benzene ring effect in the capsaicin structure) of HDPE.

[0029] In summary, the offshore photovoltaic floating material made of recyclable HDPE provided by the present invention has good anti-bite performance and corrosion resistance. DETAILED DESCRIPTION

[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Example 1

[0032] Preparation of dispersion:

[0033] A1, after 100 mL of ethanol, 0.24 mol N-hydroxymethyl acrylamide and 0.1 mol 3,5-dimethylanisole are uniformly mixed, 10 mL of 98 wt% sulfuric acid is slowly added dropwise, after the addition is complete, the temperature is raised to 35° C. The reaction is monitored by TLC plate. After the reaction is completed, a large amount of white crystals are precipitated after adding water, filtered, washed with deionized water until the filtrate is neutral, dried to obtain a crude product, and recrystallized with ethanol to obtain A2 type monomer;

[0034] A2, after 0.1 mol pentaerythritol and 100 mL tetrahydrofuran are uniformly mixed, the pH value of the mixed solution is adjusted to 10-11 (using sodium hydroxide solution), the temperature is raised to 55 ° C, 0.1 mol epoxy silane coupling agent is slowly added dropwise under stirring, and after the addition is complete, the reaction is continued for 2 hours, the reaction is stopped, the reaction is rotary evaporated, washed with water, and vacuum dried to obtain a pentaerythritol derivative, wherein the epoxy silane coupling agent is KH560;

[0035] A3, after 0.1 mol pentaerythritol derivative and 100 mL dimethyl sulfoxide are uniformly mixed, 0.3 mol potassium carbonate and 2 g potassium iodide are added under stirring, the mixture is heated to 90° C., 0.31 mol dimethylchlorosilane is slowly added dropwise, and after the addition is complete, the reaction is continued with stirring for 12 h, the reaction is stopped, the temperature is lowered, vacuum rotary evaporation is performed, and vacuum drying is performed to obtain a B3 type monomer, wherein, for the convenience of calculation, the amount of the pentaerythritol derivative is based on the amount of the added pentaerythritol in step A;

[0036] A4. After uniformly mixing 100 g of A2-type monomer, 180 g of B3-type monomer and 300 mL of toluene, the mixture was heated to 90° C. under nitrogen protection, and then 14 g of chloroplatinic acid isopropanol solution was added. The mixture was stirred at a constant temperature for 16 h. After the reaction, the platinum catalyst was adsorbed on activated carbon, the mixture was filtered, and the solvent was removed by rotary evaporation to obtain a dispersion. The mass fraction of chloroplatinic acid in the chloroplatinic acid isopropanol solution was 1%.

[0037] Example 2

[0038] Preparation of dispersion:

[0039] A1, after 100 mL of ethanol, 0.3 mol N-hydroxymethyl acrylamide and 0.1 mol 3,5-dimethylanisole are uniformly mixed, 10 mL of 98 wt% sulfuric acid is slowly added dropwise, after the addition is complete, the temperature is raised to 35°C, and the reaction is monitored by TLC plate. After the reaction is completed, a large amount of white crystals are precipitated after adding water, filtered, washed with deionized water until the filtrate is neutral, dried to obtain a crude product, and recrystallized with ethanol to obtain A2 type monomer;

[0040] A2, after 0.1 mol pentaerythritol and 100 mL tetrahydrofuran are uniformly mixed, the pH value of the mixed solution is adjusted to 10-11 (using sodium hydroxide solution), the temperature is raised to 60°C, 0.1 mol epoxy silane coupling agent is slowly added dropwise under stirring, and after the addition is complete, the reaction is continued for 2 hours, the reaction is stopped, the reaction is rotary evaporated, washed with water, and vacuum dried to obtain a pentaerythritol derivative, wherein the epoxy silane coupling agent is KH560;

[0041] A3, after 0.1 mol pentaerythritol derivative and 100 mL dimethyl sulfoxide are mixed evenly, 0.3 mol potassium carbonate and 2 g potassium iodide are added under stirring, the mixture is heated to 95° C., 0.35 mol dimethylchlorosilane is slowly added dropwise, and after the addition is complete, the reaction is continued with stirring for 12 h, the reaction is stopped, the temperature is lowered, vacuum rotary evaporation is performed, and vacuum drying is performed to obtain a B3 type monomer, wherein, for the convenience of calculation, the amount of the pentaerythritol derivative is based on the amount of the added pentaerythritol in step A;

[0042] A4. After uniformly mixing 100 g of A2-type monomer, 250 g of B3-type monomer and 300 mL of toluene, the mixture was heated to 95° C. under nitrogen protection, and then 15 g of chloroplatinic acid isopropanol solution was added. The mixture was stirred at a constant temperature for 10 h. After the reaction, the platinum catalyst was adsorbed on activated carbon, the mixture was filtered, and the solvent was removed by rotary evaporation to obtain a dispersion, wherein the mass fraction of chloroplatinic acid in the chloroplatinic acid isopropanol solution was 1%.

[0043] Example 3

[0044] Preparation of antifouling slow-release agent:

[0045] The first step is to prepare the following raw materials by weight: 20 parts of the dispersion prepared in Example 1, 10 parts of a carrier and 30 parts of mothball powder, wherein the carrier is porous carbon (the particle size of the porous carbon is 100-200 mesh, specifically 120 mesh), and the mothball powder is obtained by grinding natural mothballs through a 40-100 mesh sieve. In this embodiment, natural mothball powder through a 60 mesh sieve is selected;

[0046] The second step is to stir and mix the carrier and the mothball powder evenly, then add the dispersion, mix evenly, transfer to an extruder, extrude and granulate to obtain an antifouling slow-release agent, wherein the extrusion temperature is 170-210°C.

[0047] Example 4

[0048] Preparation of antifouling slow-release agent:

[0049] The first step is to prepare the following raw materials by weight: 30 parts of the dispersion prepared in Example 2, 20 parts of the carrier and 40 parts of mothball powder, wherein the carrier is porous carbon (the particle size of the porous carbon is 100-200 mesh, specifically 120 mesh), and the mothball powder is obtained by grinding natural mothballs through a 40-100 mesh sieve. In this embodiment, natural mothball powder through a 60 mesh sieve is selected;

[0050] The second step is to stir and mix the carrier and the mothball powder evenly, then add the dispersion, mix evenly, transfer to an extruder, extrude and granulate to obtain an antifouling slow-release agent, wherein the extrusion temperature is 170-210°C.

[0051] Comparative Example 1

[0052] Preparation of antifouling slow-release agent:

[0053] The first step is to prepare the following raw materials by weight: 20 parts of polyethylene, 10 parts of carriers and 30 parts of mothball powder, wherein the carrier is porous carbon (the particle size of the porous carbon is 100-200 mesh, specifically 120 mesh), and the mothball powder is obtained by grinding natural mothballs through a 40-100 mesh sieve. In this embodiment, natural mothball powder through a 60 mesh sieve is selected;

[0054] The second step is to stir and mix the carrier, epoxy silane coupling agent and mothball powder evenly, and then knead and granulate them.

[0055] Comparative Example 2

[0056] Preparation of antifouling slow-release agent:

[0057] The first step is to prepare the following raw materials in parts by weight: 20 parts of the dispersion prepared in Example 1 and 30 parts of mothball powder, wherein the mothball powder is natural mothballs ground through a 40-100 mesh sieve to obtain natural mothball powder selected through a 60 mesh sieve in this embodiment;

[0058] The second step is to stir and mix the carrier and the mothball powder evenly, then add the dispersion, mix evenly, transfer to an extruder, extrude and granulate to obtain an antifouling slow-release agent, wherein the extrusion temperature is 170-210°C.

[0059] Example 5

[0060] Preparation of floating materials:

[0061] Step 1: prepare the following raw materials in parts by weight: 100 parts of HDPE and 10 parts of the antifouling slow-release agent prepared in Example 3;

[0062] Step 2: After the above raw materials are mixed evenly, they are extruded through a screw extruder at 180-230°C and granulated to obtain a floating material.

[0063] Example 6

[0064] Preparation of floating materials:

[0065] Step 1: prepare the following raw materials in parts by weight: 100 parts of HDPE and 20 parts of the antifouling slow-release agent prepared in Example 4;

[0066] Step 2: After the above raw materials are mixed evenly, they are extruded through a screw extruder at 180-230°C and granulated to obtain a floating material.

[0067] Example 7

[0068] Preparation of floating materials:

[0069] Step 1: prepare the following raw materials in parts by weight: 100 parts of HDPE and 25 parts of the antifouling slow-release agent prepared in Example 3;

[0070] Step 2: After the above raw materials are mixed evenly, they are extruded through a screw extruder at 180-230°C and granulated to obtain a floating material.

[0071] Example 8

[0072] Preparation of floating materials:

[0073] Step 1: prepare the following raw materials in parts by weight: 100 parts of HDPE, 10 parts of the antifouling slow-release agent prepared in Example 3, 1 part of an anti-ultraviolet agent, and 1 part of an antioxidant; the anti-ultraviolet agent is UV-329, and the antioxidant is antioxidant 1010;

[0074] Step 2: After the above raw materials are mixed evenly, they are extruded through a screw extruder at 180-230°C and granulated to obtain a floating material.

[0075] Example 9

[0076] Preparation of floating materials:

[0077] Step 1: prepare the following raw materials in parts by weight: 100 parts of HDPE, 20 parts of the antifouling slow-release agent prepared in Example 3, 3 parts of an anti-ultraviolet agent, and 3 parts of an antioxidant; the anti-ultraviolet agent is UV-329, and the antioxidant is antioxidant 1010;

[0078] Step 2: After the above raw materials are mixed evenly, they are extruded through a screw extruder at 180-230°C and granulated to obtain a floating material.

[0079] Example 10

[0080] Preparation of floating materials:

[0081] Step 1: prepare the following raw materials in parts by weight: 100 parts of HDPE, 25 parts of the antifouling slow-release agent prepared in Example 3, 5 parts of an anti-ultraviolet agent, and 5 parts of an antioxidant; the anti-ultraviolet agent is UV-329, and the antioxidant is antioxidant 1010;

[0082] Step 2: After the above raw materials are mixed evenly, they are extruded through a screw extruder at 180-230°C and granulated to obtain a floating material.

[0083] Comparative Example 3

[0084] Preparation of floating materials:

[0085] Compared with Example 5, an equal amount of the antifouling sustained-release agent in the raw material is replaced by the antifouling sustained-release agent prepared in Comparative Example 1, and the rest is the same as Example 5.

[0086] Comparative Example 4

[0087] Preparation of floating materials:

[0088] Compared with Example 5, an equal amount of the antifouling sustained-release agent in the raw material is replaced with the antifouling sustained-release agent prepared in Comparative Example 2, and the rest is the same as Example 5.

[0089] Embodiment 11

[0090] The pellets obtained in Examples 5-10 and Comparative Examples 3-4 were subjected to the following physical property tests:

[0091] 1. Sustained release performance test:

[0092] Average sustained release rate: The pellets were made into plates and cut into 2 cm 2 The plate was placed in 100 mL of ethanol and stirred. The sample was centrifuged according to the set time and the liquid was taken out. At the same time, the concentration of mothballs in the solution was measured in a spectrophotometer. An equal amount of ethanol was added to the centrifuge tube again, and the operation steps were repeated to take the average value. See Table 1 for details.

[0093] 2. Antibacterial performance test: The tested bacteria were inoculated on the surface of the sterilized test plate, and then covered with a sterilized plastic film to make the bacteria evenly and fully contact the surface of the tested sample. The culture was kept at 37°C for 18 hours, and the number of surviving bacteria on the surface of the tested plate was calculated according to the live bacteria count on the plate, and the antibacterial rate was calculated. Among them, the negative control group was a sterilized culture dish of the same size as the surface area of ​​the tested plate; the test bacteria were marine Pseudomonas and marine Flavobacterium; the results are shown in Table 1

[0094] 3. Antifouling performance test: From July to September when marine life is growing vigorously, the pellets are made into boards and then immersed in the water of the bay. The growth of organisms attached to the contact surface between the boards and the marine water is observed every 10 days and recorded in writing. The results are shown in Table 1.

[0095] Table 1

[0096]

[0097]

[0098] From the data in Table 1, it can be seen that the floating materials obtained in Examples 5-10 have a sustained release ability for mothballs that is better than the floating materials obtained in Comparative Examples 3-4, and the antibacterial and antifouling properties of the floating materials obtained in Examples 5-10 are better than those of the floating materials obtained in Comparative Example 3.

[0099] After the pellets obtained in Examples 5-10 were made into plates, notched impact performance tests (test standard GB / T 1043.1) and flexural strength tests (test standard GB / T 9341) were performed, and the notched impact strength of Examples 5-10 was 45-60 kJ / m 2 , the bending strength is 20-26MPa.

[0100] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0101] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. An offshore photovoltaic floating material made of recyclable HDPE, characterized by: It includes the following raw materials in parts by weight: 100 parts of HDPE and 10-25 parts of antifouling slow-release agent; The antifouling slow-release agent comprises 20-30 parts of a dispersion, 10-20 parts of a carrier and 30-40 parts of mothball powder; The dispersion comprises the following steps: A1, after ethanol, N-hydroxymethyl acrylamide and 3,5-dimethylanisole are uniformly mixed, sulfuric acid is slowly added dropwise, and after the addition is complete, the temperature is raised to 30-35°C, and the reaction is monitored by TLC plate. After the reaction is completed, after post-treatment, A2 type monomer is obtained; A2. After pentaerythritol and tetrahydrofuran are uniformly mixed, the pH value of the mixed solution is adjusted to 10-11, the temperature is raised to 50-60° C., and the epoxy silane coupling agent is slowly added dropwise under stirring. After the addition is complete, the reaction is continued for 2-3 hours, the reaction is stopped, and the pentaerythritol derivative is obtained through post-treatment; A3, after the pentaerythritol derivative and dimethyl sulfoxide are uniformly mixed, potassium carbonate and potassium iodide are added under stirring, the mixture is heated to 90-95°C, dimethylchlorosilane is slowly added dropwise, and after the addition is complete, the reaction is continued under stirring for 6-12 hours, the reaction is stopped, and after post-treatment, a B3 type monomer is obtained; A4, after uniformly mixing the A2 type monomer, the B3 type monomer and toluene, heat to 90-95°C under nitrogen protection, then add chloroplatinic acid isopropanol solution, stir and react for 10-16h, and post-treat to obtain a dispersion; The molar ratio of N-hydroxymethyl acrylamide to 3,5-dimethylanisole is 2.4-3:1; The molar ratio of pentaerythritol to epoxy silane coupling agent is 1:1; The molar ratio of the pentaerythritol derivative, potassium carbonate and dimethylchlorosilane is 1:3-5:3.1-3.5; The mass ratio of the A2 type monomer to the B3 type monomer is 10:18-25.

2. The offshore photovoltaic floating material made of recyclable HDPE according to claim 1, characterized in that: The antifouling slow-release agent comprises the following steps: The carrier and the mothball powder are stirred and mixed evenly, and then the dispersion is added and mixed evenly, and then the mixture is transferred to an extruder and extruded into granules to obtain an antifouling slow-release agent.

3. The offshore photovoltaic floating material made of recyclable HDPE according to claim 2, characterized in that: The extrusion temperature of the antifouling slow-release agent is 170-210°C.

4. The offshore photovoltaic floating material made of recyclable HDPE according to claim 1, characterized in that: The mass fraction of the sulfuric acid is 98%, and the mass of H2SO4 in the sulfuric acid is 0.1-5% of the total mass of N-hydroxymethyl acrylamide and 3,5-dimethylanisole.

5. The offshore photovoltaic floating material made of recyclable HDPE according to claim 1, characterized in that: The carrier is porous adsorption particles.

6. The offshore photovoltaic floating material made of recyclable HDPE according to any one of claims 1 to 5, characterized in that: The invention also comprises the following raw materials in parts by weight: 1-5 parts of anti-ultraviolet agent and 1-5 parts of antioxidant.