A high-mechanical-performance composite material for speed reducers and its preparation method
By adding high-viscosity nylon 610, low-viscosity nylon 610, glass fiber and carbon fiber to nylon 610, combined with inorganic nanofillers, composite materials with high mechanical properties are prepared, which solves the problems of insufficient strength and high water absorption of nylon 610 and achieves better performance. Excellent mechanical properties and dimensional stability, suitable for applications such as reducers.
Patent Information
- Application Number
- CN202411111304.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-08-14
AI Technical Summary
The low strength and high water absorption of nylon 610 limit its use in applications such as reducers, especially its poor performance in dimensional stability and mechanical properties.
High-viscosity nylon 610 and low-viscosity nylon 610 are used as matrix resin and flow modifier, combined with glass fiber and carbon fiber, adding inorganic nanofillers, and using a twin-screw extruder to prepare high-mechanical performance composite materials to improve the melt index and Fiber dispersion properties prevent floating fiber phenomenon.
It significantly improves the strength and impact toughness of composite materials, improves processing performance and fiber dispersion, avoids the phenomenon of floating fibers, and improves the mechanical properties and dimensional stability of the material.
Smart Images

Figure QGIZVBXO1APE33SZ4GZMBOXGSDMR46DJEMZVSZUQ 
Figure ZFAKJSJC5W7LF5CU8PGUFNL9RC8KYGA3A7K33M8W
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nylon materials, and particularly relates to a composite material with high mechanical properties for a reducer and a preparation method thereof. Background Art
[0002] In today's highly developed science and technology, materials are gradually penetrating into every aspect of our lives, but a single material often cannot meet people's increasingly demanding requirements. One way to resolve this contradiction is to design composite materials, which contain two or more materials with different properties in their composition and achieve complementary performance.
[0003] The reducer is an important mechanical transmission device, which is widely used in various mechanical equipment in the manufacturing industry. It can reduce the speed of a high-speed rotating motor or engine to a suitable output speed and increase the torque at the same time. The main function of the reducer is to improve the mechanical transmission efficiency, reduce transmission noise, improve transmission stability, and achieve speed matching of different axes, so that mechanical equipment can work more flexibly and efficiently. Plastic parts are widely used in the fields of plastic gears, spacer rings, collars, oil pumps, etc. on reducers.
[0004] As one of the five major engineering plastics, nylon is widely used in automotive parts, electronic appliances, petrochemical and other industries due to its high mechanical strength, good wear resistance, stable chemical properties, and superior self-lubricating properties. However, nylon has disadvantages such as low mechanical properties, high water absorption, and poor dimensional stability, which affects the dimensional stability and electrical properties of the product, and its application range is greatly limited. In order to improve the performance of nylon and expand its application range, it is often modified by methods such as blocking, grafting, blending, and filling. In recent years, with the development of nanotechnology, polymer composites have received widespread attention. Compared with conventional polymer materials, polymer composites can perfectly combine the toughness, dielectric properties and rigidity, dimensional stability, thermal stability, gas-liquid barrier properties, and flame retardancy of polymers; and excellent performance can be obtained when the filling amount is very small.
[0005] Among nylon products, nylon 610 has low water absorption and excellent mechanical properties, dimensional stability and electrical insulation. Therefore, it is mainly used in products with high dimensional stability requirements, such as gears, bearings, precision parts requiring wear resistance, and electronic and electrical industries, such as computer casings, industrial electrical insulation products, cable and wire covering materials, etc. However, compared with nylon 6 and nylon 66, nylon 610 has lower strength, which limits its application. Summary of the invention
[0006] In view of the deficiencies in the prior art, the first object of the present invention is to provide a composite material with high mechanical properties for a reducer, which achieves reinforcement and toughening of nylon 610, has good surface properties, and takes into account the use requirements of strength performance and impact toughness.
[0007] The second object of the present invention is to provide a method for preparing the high mechanical property composite material for the above-mentioned reducer.
[0008] In order to achieve the first invention object, the present invention adopts the following technical solutions:
[0009] A composite material with high mechanical properties for a reducer, comprising the following components in parts by weight:
[0010] High viscosity nylon 610 50-60 parts, low viscosity nylon 610 10-20 parts, glass fiber 25-30 parts, carbon fiber 3-6 parts, inorganic nano filler 5-10 parts, compatibilizer 2-4 parts, coupling agent 1-3 parts, lubricant 1-3 parts, antioxidant 1-3 parts;
[0011] The high viscosity nylon 610 has a melt index of 5-8 g / 10 min; the low viscosity nylon 610 has a melt index of 15-20 g / 10 min; and the melt index test conditions are 230° C. and 2.16 kg.
[0012] Glass fiber is the most widely used fiber-reinforced material in fiber-reinforced polymer composites. It has low cost, light weight, good thermal stability, dimensional stability, easy processability, no moisture absorption, low dielectric constant, high tensile strength and other advantages. However, due to its fibrous structure, it has poor fluidity in the resin matrix and often has the phenomenon of floating fibers. Although reducing the viscosity of the resin can solve the above problems to a certain extent, it will lead to a decrease in the mechanical properties of the composite material. In order to solve this problem, the present invention uses high-viscosity nylon 610 as the matrix resin to exert high-strength mechanical properties; low-viscosity nylon 610 is used as a flow modifier to improve the melt index of the composite material, improve the processing performance, and improve the dispersion performance of the glass fiber. Low-viscosity nylon is of the same type as high-viscosity nylon resin, and there is no compatibility problem of ordinary flow modifiers; and low-viscosity nylon can make up for the lack of toughness of high-viscosity nylon and improve the impact strength of the composite material. Further, low-viscosity nylon 610 is 13-17 parts; when the amount of low-viscosity nylon is small, the role of the flow modifier cannot be fully exerted; when the amount of low-viscosity nylon is too much, it will affect the mechanical properties of the composite material.
[0013] Inorganic nanofillers have a small particle size and can be effectively dispersed between glass fibers and carbon fibers, which can improve fiber distribution and disperse stress. Carbon fibers are more flexible than glass fibers. Using glass fibers and carbon fibers as composite fiber modifiers can not only give full play to the rigidity of glass fibers, but also make full use of the flexibility of carbon fibers, allowing glass fibers and carbon fibers to entangle with each other. With the assistance of nanofillers, it is beneficial to improve the dispersion of glass fibers in nylon resin and prevent uneven dispersion of inorganic glass fibers and floating fiber phenomena.
[0014] Furthermore, the glass fiber is one or more of E glass fiber, C glass fiber, S glass fiber or AR glass fiber.
[0015] Furthermore, the carbon fiber is one or more of asphalt-based carbon fiber, polyacrylonitrile-based carbon fiber, and viscose-based carbon fiber.
[0016] Furthermore, the inorganic nanofiller is one or more of nano silicon dioxide, nano titanium dioxide, and nano montmorillonite.
[0017] Furthermore, the compatibilizer is one or more of PP grafted maleic anhydride, POE grafted maleic anhydride, and PE grafted maleic anhydride.
[0018] Furthermore, the coupling agent is one or more of a silane coupling agent, a titanate coupling agent, a borate coupling agent, and an aluminate coupling agent.
[0019] Furthermore, the lubricant is one or more of EBS, PETS, and silicone powder.
[0020] Furthermore, the antioxidant is one or more of hindered phenol antioxidants and phosphite antioxidants.
[0021] In order to achieve the second invention object, the present invention adopts the following technical solutions:
[0022] A method for preparing a composite material with high mechanical properties for a reducer comprises the following steps:
[0023] (1) Weighing high-viscosity nylon 610, low-viscosity nylon 610, inorganic nanofiller, compatibilizer, coupling agent, lubricant, and antioxidant components according to a ratio, mixing them to obtain a premix;
[0024] (2) The premix is added into a twin-screw extruder through a main feed port, and the glass fiber and the carbon fiber are added into the twin-screw extruder through a side feed port. The premix and the carbon fiber are melt-extruded and granulated in the twin-screw extruder to obtain a composite material with high mechanical properties for a reducer.
[0025] Furthermore, the extrusion temperature of the twin-screw extruder is controlled at 220-240° C., and the screw speed is controlled at 500-600 r / min.
[0026] Compared with the prior art, the invention has the following beneficial effects: the invention uses high-viscosity nylon 610 as the matrix resin and low-viscosity nylon 610 as the flow modifier to improve the melt index of the composite material, improve the processing performance, and improve the dispersion of the glass fiber. The use of glass fiber and carbon fiber as composite fiber modifiers can not only give play to the rigidity of the glass fiber, but also make full use of the flexibility of the carbon fiber, so that the glass fiber and the carbon fiber are entangled with each other, which is beneficial to improve the dispersion performance of the glass fiber in the nylon resin and prevent the uneven dispersion of the inorganic glass fiber and the floating fiber phenomenon. DETAILED DESCRIPTION
[0027] In order to more clearly and completely describe the technical solution of the present invention, the present invention is further described in detail by specific examples below. It should be understood that the specific examples described here are only used to explain the present invention, not to limit the present invention, and various changes can be made within the scope of the rights of the present invention. Among them, the glass fiber used in the following examples and comparative examples is E glass fiber; the carbon fiber is polyacrylonitrile-based carbon fiber; the melt index test conditions are 230°C, 2.16kg.
[0028] Example 1
[0029] A composite material with high mechanical properties for a reducer, comprising the following components in parts by weight:
[0030] 50 parts of high viscosity nylon 610, 13 parts of low viscosity nylon 610, 25 parts of glass fiber, 3 parts of carbon fiber, 5 parts of nano-silicon dioxide, 2 parts of PP grafted maleic anhydride, 1 part of KH550, 1 part of silicone powder, 1 part of antioxidant 1010;
[0031] The high viscosity nylon 610 has a melt index of 5 g / 10 min; the low viscosity nylon 610 has a melt index of 15 g / 10 min.
[0032] Example 2
[0033] A composite material with high mechanical properties for a reducer, comprising the following components in parts by weight:
[0034] High viscosity nylon 610 60 parts, low viscosity nylon 610 17 parts, glass fiber 30 parts, carbon fiber 6 parts, nano titanium dioxide 10 parts, POE grafted maleic anhydride 4 parts, KH560 3 parts, EBS 3 parts, antioxidant 168 3 parts;
[0035] The high viscosity nylon 610 has a melt index of 8 g / 10 min; the low viscosity nylon 610 has a melt index of 20 g / 10 min.
[0036] Example 3
[0037] A composite material with high mechanical properties for a reducer, comprising the following components in parts by weight:
[0038] 50 parts of high viscosity nylon 610, 17 parts of low viscosity nylon 610, 30 parts of glass fiber, 3 parts of carbon fiber, 10 parts of nano-montmorillonite, 2 parts of POE grafted maleic anhydride, 3 parts of KH550, 1 part of silicone powder, 1 part of antioxidant 1010;
[0039] The high viscosity nylon 610 has a melt index of 5 g / 10 min; the low viscosity nylon 610 has a melt index of 20 g / 10 min.
[0040] Example 4
[0041] A composite material with high mechanical properties for a reducer, comprising the following components in parts by weight:
[0042] 60 parts of high viscosity nylon 610, 13 parts of low viscosity nylon 610, 25 parts of glass fiber, 6 parts of carbon fiber, 5 parts of nano-silicon dioxide, 4 parts of POE grafted maleic anhydride, 1 part of KH550, 3 parts of silicone powder, 3 parts of antioxidant 1010;
[0043] The high viscosity nylon 610 has a melt index of 8 g / 10 min; the low viscosity nylon 610 has a melt index of 15 g / 10 min.
[0044] Example 5
[0045] A composite material with high mechanical properties for a reducer, comprising the following components in parts by weight:
[0046] 53 parts of high viscosity nylon 610, 17 parts of low viscosity nylon 610, 26 parts of glass fiber, 4 parts of carbon fiber, 7 parts of nano titanium dioxide, 3 parts of PP grafted maleic anhydride, 2 parts of KH550, 2 parts of silicone powder, 3 parts of antioxidant 1010;
[0047] The high viscosity nylon 610 has a melt index of 6 g / 10 min; the low viscosity nylon 610 has a melt index of 16 g / 10 min.
[0048] Example 6
[0049] A composite material with high mechanical properties for a reducer, comprising the following components in parts by weight:
[0050] 58 parts of high viscosity nylon 610, 14 parts of low viscosity nylon 610, 28 parts of glass fiber, 5 parts of carbon fiber, 9 parts of nano-montmorillonite, 3 parts of PP grafted maleic anhydride, 3 parts of KH550, 1 part of silicone powder, 3 parts of antioxidant 1010;
[0051] The high viscosity nylon 610 has a melt index of 7 g / 10 min; the low viscosity nylon 610 has a melt index of 18 g / 10 min.
[0052] Example 7
[0053] A composite material with high mechanical properties for a reducer, comprising the following components in parts by weight:
[0054] 55 parts of high viscosity nylon 610, 15 parts of low viscosity nylon 610, 28 parts of glass fiber, 5 parts of carbon fiber, 7 parts of nano-silicon dioxide, 3 parts of POE grafted maleic anhydride, 2 parts of KH550, 2 parts of silicone powder, 3 parts of antioxidant 1010;
[0055] The high viscosity nylon 610 has a melt index of 6 g / 10 min; the low viscosity nylon 610 has a melt index of 17 g / 10 min.
[0056] Example 8
[0057] A composite material with high mechanical properties for a reducer, comprising the following components in parts by weight:
[0058] 55 parts of high viscosity nylon 610, 10 parts of low viscosity nylon 610, 28 parts of glass fiber, 5 parts of carbon fiber, 7 parts of nano-silicon dioxide, 3 parts of POE grafted maleic anhydride, 2 parts of KH550, 2 parts of silicone powder, 3 parts of antioxidant 1010;
[0059] The high viscosity nylon 610 has a melt index of 6 g / 10 min; the low viscosity nylon 610 has a melt index of 17 g / 10 min.
[0060] Example 9
[0061] A composite material with high mechanical properties for a reducer, comprising the following components in parts by weight:
[0062] 55 parts of high viscosity nylon 610, 20 parts of low viscosity nylon 610, 28 parts of glass fiber, 5 parts of carbon fiber, 7 parts of nano-silicon dioxide, 3 parts of POE grafted maleic anhydride, 2 parts of KH550, 2 parts of silicone powder, 3 parts of antioxidant 1010;
[0063] The high viscosity nylon 610 has a melt index of 6 g / 10 min; the low viscosity nylon 610 has a melt index of 17 g / 10 min.
[0064] Comparative Example 1
[0065] A composite material with high mechanical properties for a reducer, comprising the following components in parts by weight:
[0066] 70 parts of high-viscosity nylon 610, 28 parts of glass fiber, 5 parts of carbon fiber, 7 parts of nano-silicon dioxide, 3 parts of POE grafted maleic anhydride, 2 parts of KH550, 2 parts of silicone powder, and 3 parts of antioxidant 1010; the high-viscosity nylon 610 has a melt index of 6 g / 10 min.
[0067] Comparative Example 2
[0068] A composite material with high mechanical properties for a reducer, comprising the following components in parts by weight:
[0069] 70 parts of low-viscosity nylon 610, 28 parts of glass fiber, 5 parts of carbon fiber, 7 parts of nano-silicon dioxide, 3 parts of POE grafted maleic anhydride, 2 parts of KH550, 2 parts of silicone powder, and 3 parts of antioxidant 1010; the low-viscosity nylon 610 has a melt index of 17g / 10min.
[0070] Comparative Example 3
[0071] A composite material with high mechanical properties for a reducer, comprising the following components in parts by weight:
[0072] 55 parts of high viscosity nylon 610, 15 parts of low viscosity nylon 610, 28 parts of glass fiber, 1 part of carbon fiber, 7 parts of nano-silicon dioxide, 3 parts of POE grafted maleic anhydride, 2 parts of KH550, 2 parts of silicone powder, 3 parts of antioxidant 1010;
[0073] The high viscosity nylon 610 has a melt index of 6 g / 10 min; the low viscosity nylon 610 has a melt index of 17 g / 10 min.
[0074] Comparative Example 4
[0075] A composite material with high mechanical properties for a reducer, comprising the following components in parts by weight:
[0076] 55 parts of high viscosity nylon 610, 15 parts of low viscosity nylon 610, 28 parts of glass fiber, 9 parts of carbon fiber, 7 parts of nano-silicon dioxide, 3 parts of POE grafted maleic anhydride, 2 parts of KH550, 2 parts of silicone powder, 3 parts of antioxidant 1010;
[0077] The high viscosity nylon 610 has a melt index of 6 g / 10 min; the low viscosity nylon 610 has a melt index of 17 g / 10 min.
[0078] Comparative Example 5
[0079] A composite material with high mechanical properties for a reducer, comprising the following components in parts by weight:
[0080] 55 parts of high viscosity nylon 610, 15 parts of low viscosity nylon 610, 28 parts of glass fiber, 5 parts of carbon fiber, 3 parts of POE grafted maleic anhydride, 2 parts of KH550, 2 parts of silicone powder, 3 parts of antioxidant 1010;
[0081] The high viscosity nylon 610 has a melt index of 6 g / 10 min; the low viscosity nylon 610 has a melt index of 17 g / 10 min.
[0082] The preparation process of the above embodiment is basically the same as that of the comparative example, and the specific steps are as follows:
[0083] (1) Weighing high-viscosity nylon 610, low-viscosity nylon 610, inorganic nanofiller, compatibilizer, coupling agent, lubricant, and antioxidant components according to a ratio, mixing them to obtain a premix;
[0084] (2) The premix is added into a twin-screw extruder through a main feed port, and the glass fiber and the carbon fiber are added into the twin-screw extruder through a side feed port. The composite material with high mechanical properties for a reducer is obtained by melt extrusion and granulation in the twin-screw extruder. The extrusion temperature of the twin-screw extruder is controlled at 230° C., and the screw speed is controlled at 550 r / min.
[0085] The products prepared in the above examples and comparative examples were tested for performance. The tensile performance (MPa) was tested according to ISO527 standard; the bending performance (MPa) was tested according to ISO178 standard; the notched impact strength (kJ / m 2 ) is tested according to ISO179 standard; the heat deformation temperature (℃, 1.8MPa) is tested according to ISO75 standard; and observe whether there is floating fiber on the surface of the sample.
[0086]
[0087]
[0088] As can be seen from the results of the embodiments and comparative examples in the above table, the present invention uses high-viscosity nylon 610 as the matrix resin and low-viscosity nylon 610 as the flow modifier to improve the melt index of the composite material, improve the processing performance, and improve the dispersion performance of the glass fiber. The use of glass fiber and carbon fiber as composite fiber modifiers can not only give play to the advantages of glass fiber rigidity, but also make full use of the flexibility of carbon fiber, so that the glass fiber and carbon fiber are entangled with each other, which is conducive to improving the dispersion performance of glass fiber in nylon resin and preventing inorganic glass fiber from being unevenly dispersed and floating fiber phenomenon. Comparative Example 1 does not add low-viscosity nylon, the processing performance of the composite material deteriorates, and the surface floating fiber phenomenon is serious; Comparative Example 2 lacks high-viscosity nylon, the resin bonding strength is reduced, and the mechanical properties are deteriorated. It can be seen from Comparative Examples 3-4 that when the amount of carbon fiber is too little, the mechanical properties and appearance are deteriorated; carbon fiber is not the more the better, and excessive use can easily lead to uneven fiber distribution, affecting the mechanical properties of the composite material. Comparative Example 5 does not add inorganic nanofillers, which easily leads to reduced processing performance of the composite material and poor performance.
[0089] The above description of the embodiments is to facilitate the understanding and application of the present invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the embodiments herein, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the protection scope of the present invention.
Claims
1. A composite material with high mechanical properties for reducer, It is characterized in that The composition comprises the following components in parts by weight: High viscosity nylon 610 50-60 parts, low viscosity nylon 610 10-20 parts, glass fiber 25-30 parts, carbon fiber 3-6 parts, inorganic nano filler 5-10 parts, compatibilizer 2-4 parts, coupling agent 1-3 parts, lubricant 1-3 parts, antioxidant 1-3 parts; The high viscosity nylon 610 has a melt index of 5-8 g / 10 min; the low viscosity nylon 610 has a melt index of 15-20 g / 10 min; and the melt index test conditions are 230° C. and 2.16 kg.
2. A composite material with high mechanical properties for a reducer as claimed in claim 1, It is characterized in that The glass fiber is one or more of E glass fiber, C glass fiber, S glass fiber or AR glass fiber.
3. A composite material with high mechanical properties for a reducer as claimed in claim 1, It is characterized in that The carbon fiber is one or more of asphalt-based carbon fiber, polyacrylonitrile-based carbon fiber, and viscose-based carbon fiber.
4. A composite material with high mechanical properties for a reducer as claimed in claim 1, It is characterized in that The inorganic nano filler is one or more of nano silicon dioxide, nano titanium dioxide and nano montmorillonite.
5. The composite material with high mechanical properties for a reducer as claimed in claim 1, It is characterized in that The compatibilizer is one or more of PP grafted maleic anhydride, POE grafted maleic anhydride, and PE grafted maleic anhydride.
6. A composite material with high mechanical properties for a reducer as claimed in claim 1, It is characterized in that The coupling agent is one or more of a silane coupling agent, a titanate coupling agent, a borate coupling agent, and an aluminate coupling agent.
7. A composite material with high mechanical properties for a reducer as claimed in claim 1, It is characterized in that The lubricant is one or more of EBS, PETS and silicone powder.
8. The composite material with high mechanical properties for a reducer as claimed in claim 1, It is characterized in that The antioxidant is one or more of hindered phenol antioxidants and phosphite antioxidants.
9. A method for preparing a composite material with high mechanical properties for a reducer according to any one of claims 1 to 8, It is characterized in that The following steps are involved: (1) Weighing high-viscosity nylon 610, low-viscosity nylon 610, inorganic nanofiller, compatibilizer, coupling agent, lubricant, and antioxidant components according to a ratio, mixing them to obtain a premix; (2) The premix is added into a twin-screw extruder through a main feed port, and the glass fiber and the carbon fiber are added into the twin-screw extruder through a side feed port. The premix and the carbon fiber are melt-extruded and granulated in the twin-screw extruder to obtain a composite material with high mechanical properties for a reducer.
10. A method for preparing a composite material with high mechanical properties for a reducer according to claim 9, It is characterized in that The extrusion temperature of the twin-screw extruder is controlled at 220-240° C., and the screw speed is controlled at 500-600 r / min.
Citation Information
Patent Citations
Low-warping-rate halogen-free flame retardant carbon fiber-reinforced nylon alloy material and preparation method
CN104448806A
Polyamide composite material for gas-assisted molding, and preparation method and application thereof
CN110305469A
Polyamide resin composition for semiconductor tray
CN112457662A
Polyamide resin composition and vehicle parts for holding miller and body parts for electrical equipment and appliance using the same
JP1998130494A
Cited By
High-mechanical-property composite material for speed reducer and preparation method of high-mechanical-property composite material
CN122609057A