Bottom filling glue for eliminating glue seepage, preparation method thereof and 2.5D chip packaging structure
By preparing the bottom filler containing silica and dimer acid modified epoxy resin, the problem of glue leakage in 2.5D chip packaging is solved, and communication efficiency and packaging quality are improved.
Patent Information
- Application Number
- CN202411095672.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-12
AI Technical Summary
In 2.5D chip package, underfill glue can easily lead to glue leakage, affecting the connection and communication efficiency between chips.
The bottom filler consists of silica, dimer acid modified epoxy resin, curing agent, wetting agent, carbon black and accelerator, and is prepared by stirring, centrifugal stirring, grinding and vacuum defoaming. The capillary force and wettability of the liquid inhibit the phenomenon of glue leakage.
It effectively avoids the overflow of glue, improves the communication efficiency and packaging yield of the chip, and ensures the fullness of the gap and dimensional stability.
Smart Images

Figure CN118620563B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chip packaging, and in particular relates to a bottom filling glue for eliminating glue seepage, a preparation method thereof and a 2.5D chip packaging structure. Background Art
[0002] 2.5D packaging technology is a packaging technology that can realize homogeneous or heterogeneous integration of multiple chips. It integrates multiple bare chips on a silicon interposer to achieve high-speed interconnection and short-distance communication between chips. The silicon interposer has high-density, high-performance interconnection characteristics, which can greatly improve the overall performance of the system. However, in 2.5D packaging technology, when the gap between chips is filled with bottom filling glue, glue penetration is prone to occur, affecting the connection and communication between chips.
[0003] Therefore, how to provide a bottom filling glue to suppress the glue seepage phenomenon in the 2.5D chip packaging, so as to improve the communication efficiency of the chip, is a technical problem that technical personnel in this field need to solve urgently. Summary of the invention
[0004] The object of the present invention is to provide a bottom filling glue that eliminates glue seepage, a preparation method thereof and a 2.5D chip packaging structure, so as to solve at least one of the above-mentioned technical problems.
[0005] To achieve the above-mentioned purpose, the first aspect of the present invention provides a bottom filling glue for eliminating glue seepage, wherein the bottom filling glue comprises the following components by mass percentage: 55% to 65% of silicon dioxide, 19% to 23% of dimer acid-modified epoxy resin, 16% to 21% of curing agent, 0.1% to 0.5% of wetting agent, 0.1% to 0.3% of carbon black and 0.1% to 0.3% of accelerator.
[0006] In the first aspect, the mass percentage of the lubricant is 0.3%, the mass percentage of the carbon black is 0.1%, and the mass percentage of the accelerator is 0.2%.
[0007] In the first aspect, the type of the wetting agent comprises BYK-220S.
[0008] In the first aspect, the curing agent includes at least one of a tertiary amine-terminated hyperbranched polymer and an epoxythiol curing agent.
[0009] In the first aspect, the average particle size of the silicon dioxide is 2 to 6 μm.
[0010] In a first aspect, the accelerator comprises benzothiazole.
[0011] In the first aspect, the dimer acid-modified epoxy resin includes at least one of EPD-172 and ZT-5251DA.
[0012] A second aspect of the present invention provides a method for preparing the bottom filling glue for eliminating glue seepage as described in the first aspect, the preparation method comprising:
[0013] S1. Add each component into a stirring cup according to their respective mass percentages, stir and mix, and obtain a first slurry, wherein the mass percentages of the components specifically include: 55% to 65% silicon dioxide, 19% to 23% dimer acid-modified epoxy resin, 16% to 21% curing agent, 0.1% to 0.5% wetting agent, 0.1% to 0.3% carbon black, and 0.1% to 0.3% accelerator;
[0014] S2, transferring the first slurry into a first centrifugal mixer, stirring and mixing, to obtain a second slurry;
[0015] S3, transferring the second slurry to a three-roll mill for dispersion treatment to obtain a uniformly dispersed third slurry;
[0016] S4, transferring the third slurry into a second centrifugal mixer for vacuum degassing to obtain bottom filling glue.
[0017] In the second aspect, in S2, the working parameters of the first centrifugal mixer include: stirring and mixing time of 120 to 250 s, rotation of 850 r / min, and revolution of 1000 r / min; in S3, the working parameters of the three-roll grinder include: feeding gap of 8 to 13 μm, and discharging gap of 3 to 7 μm; in S4, the working parameters of the second centrifugal mixer include: vacuum degassing time of 40 to 60 s, rotation of 850 r / min, and revolution of 1000 r / min.
[0018] The third aspect of the present invention provides a 2.5D chip packaging structure, which includes: a PCB substrate; a plurality of C4 bumps, which are spaced apart on the upper surface of the PCB substrate; a silicon interposer, which is penetrated by a plurality of through silicon vias, each of which is connected to a corresponding C4 bump; a gap between the silicon interposer and the PCB substrate is filled with a bottom filling material; a rewiring layer, which is arranged on the upper surface of the silicon interposer; a plurality of chips, which are spaced apart above the rewiring layer, each of which is electrically connected to the rewiring layer through a plurality of micro bumps; and a gap between the plurality of chips and the rewiring layer is filled with the bottom filling glue for eliminating glue seepage as described in the first aspect.
[0019] Beneficial Effects
[0020] The invention provides a bottom filling glue for eliminating glue seepage, which comprises the following components by mass percentage: 55% to 65% of silicon dioxide, 19% to 23% of dimer acid modified epoxy resin, 16% to 21% of curing agent, 0.1% to 0.5% of wetting agent, 0.1% to 0.3% of carbon black and 0.1% to 0.3% of accelerator; the dimer acid modified epoxy resin is semi-solid at room temperature and has certain fluidity after heating, the mechanical strength of the bottom filling glue is enhanced by adding silicon dioxide, and the curing degree and curing time of the bottom filling glue are controlled in combination with the curing agent and the accelerator, and the wettability of the bottom filling glue is further adjusted by adding the wetting agent, so as to achieve the purpose of inhibiting glue seepage; in addition, the bottom filling glue formed by using the dimer acid modified epoxy resin as a matrix material has good dimensional stability, and the dimensional shrinkage rate is small after curing. The bottom filling glue prepared by the formula ratio of the present invention has weaker capillary force and stronger silicon wafer wettability. When filling the gap between the chip and the rewiring layer in the 2.5D chip packaging structure, it can prevent the glue from overflowing from the gap between two adjacent chips, thereby achieving the purpose of inhibiting glue seepage in the 2.5D chip packaging process, while improving the communication efficiency and packaging yield of the chip. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of this specification or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figure 1 There are four situations where glue is filled in the gap between two adjacent chips;
[0023] Figure 2 A flow chart of a method for preparing a bottom filling adhesive for eliminating adhesive seepage provided by the present invention;
[0024] Figure 3 A schematic diagram of a 2.5D chip packaging structure provided by the present invention;
[0025] Figure 4 It is a structural schematic diagram of the capillary force testing device in the present invention;
[0026] Reference numerals:
[0027] 1. PCB substrate; 2. C4 bump; 3. Bottom filling material; 4. Silicon interposer; 5. Through silicon via; 6. Rewiring layer; 7. Chip; 8. Micro bump;
[0028] C1, 0.5 mm capillary; C2, bottom filling glue; C3, glass slide; C0, 110°C electric heating plate. DETAILED DESCRIPTION
[0029] The present invention will be described in detail below in conjunction with specific implementations and examples, and the advantages and various effects of the present invention will be more clearly presented. It should be understood by those skilled in the art that these specific implementations and examples are used to illustrate the present invention, rather than to limit the present invention.
[0030] Throughout the specification, unless otherwise specifically stated, the terms used herein should be understood as meanings commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. In the event of a conflict, the present specification takes precedence.
[0031] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or obtained by existing methods.
[0032] The general idea of the present invention is as follows:
[0033] In 2.5D chip packaging, the gap between two adjacent chips is small. When the bottom filler is filled between the chip and the rewiring layer, the glue will climb up from the gap between the two chips and penetrate into the surface of the chip under the influence of capillary force, which is the phenomenon of glue seepage. Four situations may occur in this process, such as Figure 1 Shown: In Figure 1 In (a), the capillary force of the glue in the chip gap is weak, and the wettability with the silicon wafer is poor (manifested by the large contact angle of the glue on the silicon surface). At this time, the glue climbs to a low height, presenting a convex liquid surface, and no glue seepage occurs. Figure 1 In (b), the capillary force of the glue in the chip gap is weak, and the wettability with the silicon wafer is strong (manifested by the small contact angle of the glue on the silicon surface). At this time, the glue climbs to a low height, presenting a concave liquid surface, and no glue seepage occurs. Figure 1 In (c), the glue has a strong capillary force in the chip gap and poor wettability with the silicon wafer (manifested by a large contact angle of the glue on the silicon surface). At this time, the glue climbs high and presents a convex liquid surface, which may cause glue seepage. Figure 1In (d), the glue has a strong capillary force in the chip gap and has strong wettability with the silicon wafer (manifested by a small contact angle of the glue on the silicon surface). At this time, the glue climbs to a high height and presents a concave liquid surface, and glue seepage will occur; among them, the convex liquid surface is more prone to glue seepage than the concave liquid surface. Therefore, as long as the capillary action of the glue is appropriately weakened and the wettability with the silicon wafer is enhanced, the glue seepage phenomenon can be effectively suppressed. In addition, when the capillary action is too weak, the fluidity of the glue will deteriorate and it will not be able to fill the gap. If it is too strong, glue seepage will easily occur; the stronger the wettability with the silicon wafer, not only can the glue present a concave liquid surface, but also the glue can make the contact with the micro-bumps at the bottom of the chip more sufficient, thereby enhancing its reliability. Based on this, the present invention provides a bottom filling glue with weak capillary action and strong wettability to avoid glue seepage during 2.5D chip packaging.
[0034] The present application provides a bottom filling glue for eliminating glue seepage, and the bottom filling glue includes the following components in mass percentage: 55% to 65% silicon dioxide, 19% to 23% dimer acid-modified epoxy resin, 16% to 21% curing agent, 0.1% to 0.5% wetting agent, 0.1% to 0.3% carbon black and 0.1% to 0.3% accelerator.
[0035] Specifically, the present invention provides a bottom filling glue for eliminating glue seepage, which includes the following components in mass percentage: 55% to 65% of silicon dioxide, 19% to 23% of dimer acid modified epoxy resin, 16% to 21% of curing agent, 0.1% to 0.5% of wetting agent, 0.1% to 0.3% of carbon black and 0.1% to 0.3% of accelerator; the dimer acid modified epoxy resin is semi-solid at room temperature and has a certain fluidity after heating, and the mechanical strength of the bottom filling glue is enhanced by adding silicon dioxide, and the curing degree and curing time of the bottom filling glue are controlled in combination with the curing agent and the accelerator, and the wettability of the bottom filling glue is further adjusted by adding the wetting agent, so as to achieve the purpose of inhibiting glue seepage; in addition, the bottom filling glue formed by using the dimer acid modified epoxy resin as the matrix material has good dimensional stability, and after curing, the dimensional shrinkage rate is small. The bottom filling glue prepared by the formula ratio of the present invention has weaker capillary force and stronger silicon wafer wettability. When filling the gap between the chip and the rewiring layer in the 2.5D chip packaging structure, it can prevent the glue from overflowing from the gap between two adjacent chips, thereby achieving the purpose of inhibiting glue seepage in the 2.5D chip packaging process, while improving the communication efficiency and packaging yield of the chip.
[0036] In some possible embodiments, the mass percentage of the lubricant is 0.3%, the mass percentage of the carbon black is 0.1%, and the mass percentage of the accelerator is 0.2%.
[0037] Those skilled in the art will appreciate that in order to study the effect of the ratio of epoxy resin, curing agent and filling material on the performance of the bottom filling adhesive, the ratio of lubricant, carbon black and accelerator is controlled and the addition percentage is fixed.
[0038] In some possible embodiments, the wetting agent includes BYK-220S.
[0039] This is because the wetting agent is used to improve the wettability between the bottom filling glue and the silicon chip, so that the glue liquid presents a concave liquid surface between two adjacent chips to inhibit the glue seepage phenomenon. In a specific embodiment, the present invention uses a low molecular weight unsaturated acidic polycarboxylic acid polyester solution (BYK-220S) containing a polysiloxane copolymer as a wetting agent. BYK-220S can improve the dispersibility of silicon dioxide in the bottom filling glue and avoid the sedimentation of silicon dioxide; at the same time, because BYK-220S contains a small amount of polysiloxane copolymer, it can improve the floating color phenomenon and enhance the surface smoothness and leveling of the bottom filling glue.
[0040] In some possible embodiments, the curing agent includes at least one of a tertiary amine-terminated hyperbranched polymer and an epoxythiol curing agent.
[0041] Those skilled in the art can understand that the curing agent is used to react with the epoxy resin to convert the fluid state of the bottom filling glue into a solid state. The dimer acid-modified epoxy resin used in the present application, in order to control the reaction rate, in a specific embodiment, a terminal tertiary amine hyperbranched polymer or an epoxythiol curing agent can be used as a curing agent to improve the performance of the bottom filling glue, wherein the terminal tertiary amine hyperbranched polymer can be selected as QNP1, and the epoxythiol curing agent can be selected as YHY-4300.
[0042] In some possible embodiments, the average particle size of the silicon dioxide is 2 to 6 μm.
[0043] In order to control the flow speed of the glue in the gap flow process, silicon dioxide with an average particle size of 2 to 6 μm is selected as the filling material of the bottom filling glue.
[0044] In some possible embodiments, the accelerator includes benzothiazole.
[0045] Those skilled in the art can understand that the promoter of the present application is equivalent to a catalyst for the reaction, which can promote the reaction at a certain temperature and increase the reaction rate. In a specific embodiment, benzothiazole is used as the promoter in the present application.
[0046] In some possible embodiments, the model of the dimer acid-modified epoxy resin includes at least one of EPD-172 and ZT-5251DA.
[0047] This is because the general structural formula of dimer acid modified epoxy resin is:
[0048]
[0049] Here, R is an alkyl group having 1 to 20 carbon atoms.
[0050] In this application, the preferred models of dimer acid epoxy resin are EPD-172 and ZT-5251DA. EPD-172 is an adduct of bisphenol A epoxy resin and dibasic fatty acid. At room temperature, it has a high viscosity and requires appropriate heating to assist flow or suction. The introduction of fatty acids into the main chain of bisphenol A epoxy resin can give the bottom filling glue a certain degree of flexibility. AZT-5251DA is a low-halogen, low-viscosity dimer acid modified epoxy resin that can improve the strength and flexibility of the bottom filling glue.
[0051] Based on a general inventive concept, the second aspect of the present invention provides a method for preparing a bottom filling glue that eliminates glue seepage, such as Figure 2 As shown, the preparation method comprises:
[0052] S1. Add each component into a stirring cup according to their respective mass percentages, stir and mix, and obtain a first slurry, wherein the mass percentages of the components specifically include: 55% to 65% silicon dioxide, 19% to 23% dimer acid-modified epoxy resin, 16% to 21% curing agent, 0.1% to 0.5% wetting agent, 0.1% to 0.3% carbon black, and 0.1% to 0.3% accelerator;
[0053] S2, transferring the first slurry into a first centrifugal mixer, stirring and mixing, to obtain a second slurry;
[0054] S3, transferring the second slurry to a three-roll mill for dispersion treatment to obtain a uniformly dispersed third slurry;
[0055] S4, transferring the third slurry into a second centrifugal mixer for vacuum degassing to obtain bottom filling glue.
[0056] As another optional embodiment, in S2, the working parameters of the first centrifugal mixer include: stirring and mixing time of 120 to 250 s, rotation of 850 r / min, and revolution of 1000 r / min; in S3, the working parameters of the three-roll grinder include: feeding gap of 8 to 13 μm, and discharging gap of 3 to 7 μm; in S4, the working parameters of the second centrifugal mixer include: vacuum degassing time of 40 to 60 s, rotation of 850 r / min, and revolution of 1000 r / min.
[0057] Based on a general inventive concept, the third aspect of the present invention provides a 2.5D chip packaging structure, such as Figure 3 As shown, the 2.5D chip packaging structure includes: a PCB substrate 1; a plurality of C4 bumps 2, wherein the plurality of C4 bumps 2 are arranged at intervals on the upper surface of the PCB substrate 1; a silicon interposer 4, wherein the silicon interposer 4 is penetrated by a plurality of through silicon vias 5, wherein each of the through silicon vias 5 is connected to a corresponding one of the C4 bumps 2; a gap between the silicon interposer 4 and the PCB substrate 1 is filled with a bottom filling material 3; a rewiring layer 6, wherein the rewiring layer 6 is arranged on the upper surface of the silicon interposer 4; a plurality of chips 7, wherein the plurality of chips 7 are arranged at intervals above the rewiring layer 6, wherein each of the chips 7 and the rewiring layer 6 is electrically connected via a plurality of micro bumps 8; and a bottom filling glue for eliminating glue seepage as described in the first aspect is filled between the plurality of chips 7 and the rewiring layer 6.
[0058] Specifically, in a 2.5D chip packaging structure, the rewiring layer 6 contains a circuit structure, and signals are transmitted by connecting to the micro-bumps 8. The chip 7 is fixedly connected to the micro-bumps 8, so that there is a gap between the chip 7, the rewiring layer 6 and the micro-bumps 8. Glue is dripped on the rewiring layer 6 on one side of one of the chips 7. Driven by the kinetic energy of the glue, the glue flows from one side of a chip 7 into the gap between the micro-bumps 8, and then flows into the gap between the next chip 7 and the micro-bumps 8. During the flow of the glue, due to capillary action, the glue will creep into the gap between two adjacent chips 7. If the height of the glue creeping is too high, it will cause glue seepage, affecting the communication efficiency of the chip. When the glue of the bottom filling glue prepared in the present application is used for filling, glue seepage will not occur.
[0059] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0060] The components of the bottom filling glue in Comparative Examples 1-6 and Examples 1-4 are shown in Table 1 according to mass percentage:
[0061] Table 1 Raw material components by mass percentage
[0062]
[0063] The capillary action test and wettability test of the bottom filling glue provided in Examples 1-4 and Comparative Examples 1-6 are performed. The specific test process is as follows:
[0064] 1. Test method of capillary action test: Place a glass slide on a hot plate with a measured temperature of 110℃, apply 1g of glue on the glass slide, and then vertically place one end of a capillary with an inner diameter of 0.5mm on the surface of the glue, wait for 20 minutes, and measure its climbing height with a ruler. The test device is as follows: Figure 4 shown.
[0065] 2. Wettability test method: Use a contact angle tester to test the contact angle of the glue on a 110°C substrate.
[0066] The test results are shown in Table 2 below:
[0067] Table 2 Test results
[0068]
[0069] From the above table, we can see that:
[0070] (1) Comparative Example 1 uses bisphenol A epoxy resin as the base material. When the bottom filling glue prepared fills the gap, due to the strong capillary action and wettability of the glue liquid, the glue creeping height is high, the contact angle is large, and a convex liquid surface is presented, resulting in glue seepage;
[0071] (2) In comparative example 2, the bottom filling glue prepared by using an anhydride curing agent methyltetrahydrophthalic anhydride has a high creeping height and a large contact angle when filling the gap, due to the strong capillary action and wettability of the glue, presenting a convex liquid surface and causing glue seepage;
[0072] (3) In comparative example 3, no wetting agent was added, and the contact angle was the largest, which made it easier to form a convex liquid surface, causing glue seepage. It can be seen that the wetting agent can adjust the contact angle of the bottom filling glue liquid, and then adjust the liquid surface of the glue liquid of two adjacent chips by controlling the addition ratio;
[0073] (4) The addition ratio of dimer acid-modified epoxy resin and curing agent in Comparative Examples 4-6 exceeds the formula ratio of the present application. When filling the gap, the prepared bottom filling glue has a high glue creeping height and a large contact angle, which is prone to glue seepage;
[0074] (5) The bottom filling glue prepared by using the dimer acid-modified epoxy resin and the curing agent in the prescribed formula ratio in Examples 1-4 has a low creeping height and a small contact angle when filling the gap, and will not cause glue seepage. The bottom filling glue can fill the gap. The bottom filling glue has strong stability, small dimensional shrinkage, and will not have voids after curing.
[0075] Finally, it should be noted that the terms "comprises," "includes," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements that are inherent to such process, method, article, or apparatus.
[0076] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0077] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A bottom filling glue for eliminating glue seepage, characterized in that: The bottom filling glue comprises the following components by mass percentage: 55% to 65% silicon dioxide, 19% to 23% dimer acid modified epoxy resin, 16% to 21% curing agent, 0.1% to 0.5% wetting agent, 0.1% to 0.3% carbon black and 0.1% to 0.3% accelerator; The model of the wetting agent is BYK-220S; The curing agent is at least one of a terminal tertiary amine hyperbranched polymer and an epoxy mercaptan curing agent; The average particle size of the silicon dioxide is 2 to 6 μm; The accelerator is benzothiazole; The model of the dimer acid modified epoxy resin is EPD-172.
2. The bottom filling glue for eliminating glue seepage according to claim 1, characterized in that: The mass percentage of the wetting agent is 0.3%, the mass percentage of the carbon black is 0.1%, and the mass percentage of the accelerator is 0.2%.
3. A method for preparing a bottom filling adhesive for eliminating adhesive seepage according to any one of claims 1 to 2, characterized in that: The preparation method comprises: S1. Add each component into a stirring cup according to their respective mass percentages, stir and mix, and obtain a first slurry, wherein the mass percentages of the components specifically include: 55% to 65% silicon dioxide, 19% to 23% dimer acid-modified epoxy resin, 16% to 21% curing agent, 0.1% to 0.5% wetting agent, 0.1% to 0.3% carbon black, and 0.1% to 0.3% accelerator; S2, transferring the first slurry into a first centrifugal mixer, stirring and mixing, to obtain a second slurry; S3, transferring the second slurry to a three-roll mill for dispersion treatment to obtain a uniformly dispersed third slurry; S4, transferring the third slurry into a second centrifugal mixer for vacuum degassing to obtain a bottom filling glue; In S2, the working parameters of the first centrifugal mixer include: stirring and mixing time of 120 to 250 seconds, rotation of 850 r / min, and revolution of 1000 r / min; In S3, the working parameters of the three-roll mill include: the feed gap is 8 to 13 μm, the discharge gap is 3 to 7 μm; In S4, the working parameters of the second centrifugal mixer include: vacuum degassing time of 40 to 60 seconds, rotation of 850 r / min, and revolution of 1000 r / min.
4. A 2.5D chip packaging structure, characterized in that: The 2.5D chip packaging structure includes: PCB substrate; A plurality of C4 bumps, wherein the plurality of C4 bumps are arranged at intervals on the upper surface of the PCB substrate; A silicon interposer, wherein a plurality of through silicon vias are provided through the silicon interposer, each of the through silicon vias is connected to a corresponding one of the C4 bumps; and a gap between the silicon interposer and the PCB substrate is filled with a bottom filling material; a rewiring layer, the rewiring layer being disposed on an upper surface of the silicon interposer; A plurality of chips are arranged above the rewiring layer at intervals, and each of the chips is electrically connected to the rewiring layer via a plurality of micro-bumps; and the bottom filling glue for eliminating glue seepage as described in any one of claims 1-2 is filled between the plurality of chips and the rewiring layer.