Modified clay for roadbed and preparation method and application thereof

By mixing industrial waste residue-furfural residue with low liquid limit clay after pretreatment and purification to form modified clay, the stability problem of low liquid limit soil in roadbed filling is solved, and efficient soil solidification and environmentally friendly soil are achieved. Subgrade material preparation.

CN118620632BActive Publication Date: 2024-10-22UNIV OF JINAN +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411117441.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-10-22
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

The low liquid limit soil used in traditional roadbed filling can easily lead to uneven settlement, cracking and sliding problems, and the production of traditional curing agents consumes a lot of resources and emits harmful substances, polluting the environment.

Method used

Industrial waste residue - furfural residue is used as a solidifying agent. After pretreatment and purification, it is mixed with low liquid limit clay, and water or phosphoric acid aqueous solution is added to form modified clay, which is used to solidify low liquid limit soil and improve the strength and stability of the soil.

Benefits of technology

It improves the unconfined compressive strength, shear strength and expansion resistance of low liquid limit soil, reduces environmental pollution, realizes the reuse of industrial waste residue, and provides an economical and environmentally friendly solution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118620632B_ABST
    Figure CN118620632B_ABST
Patent Text Reader

Abstract

The present invention discloses a modified clay for roadbed and a preparation method and application thereof, belonging to the technical field of soil solidification. The modified clay for roadbed is composed of low liquid limit clay, a curing agent and water; the curing agent is pretreated furfural residue, purified furfural residue, a mixture of pretreated furfural residue and phosphoric acid aqueous solution, or a mixture of purified furfural residue and phosphoric acid aqueous solution. The present invention preliminarily assigns values ​​to four mechanical tests of unconfined strength, shear strength, shrinkage resistance and expansion resistance of the modified clay for roadbed, and completes a comprehensive evaluation of low liquid limit clay with different dosages of soil curing agents. The present invention fully considers the low cost of using curing agents and the purpose of environmental protection and turning waste into treasure, as well as the excellent curing effect on low liquid limit clay.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of soil solidification, in particular to modified clay for roadbed and a preparation method and application thereof. Background Art

[0002] With the continuous expansion of urbanization, more and more civil engineering structures, such as railway / highway subgrades, foundations and embankments, are inevitably built on problematic soils, which will bring safety and reliability problems to the structure if not improved or stabilized. Soil stabilizers have been widely used as an effective and reliable technology to solve problems such as slope stability, pavement bearing capacity, embankment bearing capacity, earthquake liquefaction and foundation bearing capacity.

[0003] If low liquid limit soil is used for roadbed filling, it is easy to cause engineering problems such as uneven settlement, cracking, and sliding, so it cannot be directly used for roadbed filling. At present, low liquid limit soil for engineering is mainly improved by traditional curing agents such as cement, lime, and fly ash. These curing agents undergo a series of physical and chemical reactions with soil particles, improving the engineering properties of the soil by changing the particle composition and mineral composition of the soil.

[0004] However, traditional curing agents also have some negative effects. For example, the strong alkaline environment formed by inorganic curing agents will pollute the surrounding soil and groundwater. Most modified clays are brittle soils, which are not conducive to the stability of the roadbed under traffic loads. In addition, the production of cement and lime not only consumes a large amount of limestone, clay, electricity, and heat energy, but also emits harmful substances that affect air quality, such as CO2, SO2, dust, etc.

[0005] Therefore, as people pay more and more attention to environmental issues, it is particularly important to design a low liquid limit curing agent that is both economical and environmentally friendly. Summary of the invention

[0006] In order to solve the problems existing in the prior art, the present invention provides a modified clay for roadbed and a preparation method and application thereof; the present invention can be used to solidify low liquid limit soil by reasonably selecting industrial waste residue-furfural residue material, and performing preliminary drying and screening treatment, so as to achieve the purpose of turning industrial waste residue into treasure.

[0007] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0008] On the one hand, the present invention provides a modified clay for roadbed, which is composed of the following components: low liquid limit clay, a curing agent and water; the curing agent is pretreated furfural residue, purified furfural residue, a mixture of pretreated furfural residue and phosphoric acid aqueous solution, or a mixture of purified furfural residue and phosphoric acid aqueous solution.

[0009] Preferably, the pretreated furfural residue is purchased furfural residue, which is first crushed, passed through a 0.5 mm sieve, and then dried in an oven to constant weight, and then sieved with a sieve with an aperture of 0.5 mm to obtain the pretreated furfural residue.

[0010] Further, the purified furfural residue is obtained by the following steps:

[0011] 1) Put the purchased furfural residue into the filter bag and rinse it with water at a flow rate of about 0.8 m / s for 12 hours; the filter bag is a PP double-layer filter bag with a filtration accuracy of 0.1-50 microns;

[0012] 2) drying the washed furfural residue in an oven at a temperature of 80-200°C;

[0013] 3) The dried furfural residue is sieved using a sieve with a pore size of 0.5 mm to obtain purified furfural residue.

[0014] Preferably, the modified clay for roadbed is composed of the following components in parts by weight: 100 parts by weight of low liquid limit clay; 6-20 parts by weight of pretreated furfural residue; and 21 parts by weight of water.

[0015] Preferably, the modified clay for roadbed is composed of the following components in parts by weight: 100 parts by weight of low liquid limit clay; 6-18 parts by weight of pretreated furfural residue; 2-15 parts by weight of phosphoric acid aqueous solution; 7.5-19.2 parts by weight of water; wherein the mass ratio of the phosphoric acid aqueous solution to the pretreated furfural residue is 1:1-3; the concentration of the phosphoric acid aqueous solution is 10wt%;

[0016] The total moisture content of the modified clay for roadbed is 21 parts by weight.

[0017] Preferably, the modified clay for roadbed is composed of the following components in parts by weight: 100 parts by weight of low liquid limit clay; 3-20 parts by weight of purified furfural residue; and 21 parts by weight of water.

[0018] Preferably, the modified clay for roadbed is composed of the following components in parts by weight: 100 parts by weight of low liquid limit clay; 3-18 parts by weight of purified furfural slag; 2-15 parts by weight of phosphoric acid aqueous solution; 7.5-19.2 parts by weight of water; the mass ratio of the phosphoric acid aqueous solution to the purified furfural slag is 1:1-3; the concentration of the phosphoric acid aqueous solution is 10wt%;

[0019] The total moisture content of the modified clay for roadbed is 21 parts by weight.

[0020] The low liquid limit clay of the present invention has a soil particle size (≤0.075 mm) of ≥50%, a liquid limit wl≤50%, and a plasticity index Ip>7.

[0021] On the other hand, the present invention also provides a method for preparing the modified clay for roadbed, which comprises firstly mechanically stirring and mixing the low liquid limit clay and the curing agent evenly, then adding water and stirring evenly.

[0022] On the other hand, the present invention also provides an application of the modified clay for roadbed, which can be used as different grades of highway base or subbase according to the unconfined compressive strength of the prepared modified clay.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The industrial waste residue-furfural residue selected by the present invention contains a large amount of lignin and cellulose. Lignin and cellulose play a major role in the solidification of low liquid limit clay by industrial waste residue-furfural residue. On the one hand, lignin produces a gelling substance when mixed with water, and the double electric layer in the low liquid limit clay is thinned by filling and bonding with lignin, thereby achieving the purpose of enhancing the strength of the soil. On the other hand, cellulose provides additional interlocking and bridging effects, and the adsorption of fine particles and water by the fiber achieves the purpose of solidifying the low liquid limit soil. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The unconfined compressive strength diagram of modified clay at different pre-treated furfural residue dosages; wherein the pre-treated furfural residue dosage is the percentage of the pre-treated furfural residue weight to the low liquid limit clay weight;

[0026] Figure 2 The graphs are the cohesion and internal friction angle of modified clay at different pre-treated furfural residue dosages; where the pre-treated furfural residue dosage is the percentage of the pre-treated furfural residue weight to the low liquid limit clay weight;

[0027] Figure 3 The figure is the shrinkage rate of modified clay under different pre-treated furfural residue dosages; where es is the linear shrinkage rate; ev is the volume shrinkage rate; where the pre-treated furfural residue dosage is the percentage of the pre-treated furfural residue weight to the low liquid limit clay weight;

[0028] Figure 4 The figure is a graph of the no-load expansion rate of modified clay under different pre-treated furfural residue dosages; wherein the pre-treated furfural residue dosage is the percentage of the pre-treated furfural residue weight to the low liquid limit clay weight;

[0029] Figure 5 The unconfined compressive strength diagram of modified clay compounded with different amounts of phosphoric acid and 15% furfural residue; where the phosphoric acid content is the percentage of the weight of phosphoric acid to the weight of low liquid limit clay;

[0030] Figure 6The unconfined compressive strength diagram of the modified clay at 105°C (Example 15), 150°C (Example 30), and 200°C (Example 31) for purification of furfural residue with a dosage of 3%;

[0031] Unconfined compressive strength diagram of modified clay at 105°C (Example 17), 150°C (Example 32), and 200°C (Example 33) when the purified furfural residue dosage is 9%;

[0032] Unconfined compressive strength of modified clay at 105°C (Example 19), 150°C (Example 34), and 200°C (Example 35) when the purified furfural residue content is 15%

[0033] The dosage of the purified furfural residue is the percentage of the weight of the purified furfural residue to the weight of the low liquid limit clay. DETAILED DESCRIPTION

[0034] In order to make the technical problems to be solved, technical solutions and advantages of the present invention more clear, a detailed description will be given below with reference to the accompanying drawings and specific embodiments.

[0035] In the present invention, the materials and reagents used are commercially available unless otherwise specified. The concentration of the phosphoric acid aqueous solution is 10wt%. The double-layer filter bag is a PP double-layer filter bag with a filtration accuracy of 0.1-50 microns; furfural residue: purchased from Binzhou Huitong Bioenergy Co., Ltd.; the low liquid limit clay used in the present invention: the soil particles with a particle size (≤0.075 mm) are 94.9%, the natural water content w is 9.2%, the liquid limit wl is 39.5%, the plasticity index Ip is 12.6, and the maximum dry density is 1.63 g / cm 3 , the optimal moisture content is 21.0%.

[0036] The present invention provides modified clay for roadbed and a preparation method and application thereof, and specific embodiments are as follows.

[0037] A modified clay for roadbed is composed of the following components by weight: 100 parts by weight of low liquid limit clay; 6-20 parts by weight of pretreated furfural residue; and 21 parts by weight of water. Specific embodiments are as follows.

[0038] Example 1

[0039] A modified clay for roadbed consists of the following components in percentage by weight: 100 parts by weight of low liquid limit clay; 6 parts by weight of pretreated furfural residue; and 21 parts by weight of water.

[0040] The pretreated furfural residue was prepared by the following method: the purchased furfural residue was first crushed and passed through a 0.5 mm sieve, at which time the moisture content was 42.6%, and then dried in an oven at a temperature of 105°C for 24 h, and then the dried furfural residue was sieved using a sieve with an aperture of 0.5 mm.

[0041] The method for preparing the modified clay for roadbed is: firstly mechanically stir and mix the low liquid limit clay and the curing agent evenly, then add water and stir evenly.

[0042] Embodiment 2-6

[0043] The substances and amounts of modified clay for roadbed in Examples 2-6 are shown in Table 1, and the other conditions are the same as in Example 1.

[0044] Table 1

[0045]

[0046] In order to further illustrate the beneficial effects of the present invention, the following comparative example was constructed.

[0047] Comparative Example 1

[0048] In this comparative example, 100 parts by weight of low liquid limit clay and 21 parts by weight of water were used, and the rest was the same as in Example 1.

[0049] Comparative Example 2

[0050] In this comparative example, 100 parts by weight of low liquid limit clay, 3 parts by weight of pretreated furfural residue, and 21 parts by weight of water are used, and the rest is the same as in Example 1.

[0051] Comparative Example 3

[0052] In this comparative example, the pretreated furfural residue was replaced with an equal amount of cement (ordinary Portland cement: PO 42.5), and the other conditions were the same as those in Example 4.

[0053] Comparative Example 4

[0054] In this comparative example, the pretreated furfural residue was replaced with an equal amount of lime powder, and the other conditions were the same as those in Example 4.

[0055] Comparative Example 5

[0056] In this comparative example, the pretreated furfural residue was replaced with an equal amount of lignin, and the other conditions were the same as in Example 4.

[0057] Comparative Example 6

[0058] In this comparative example, the pretreated furfural residue was replaced with an equal amount of cellulose (18 mm in length), and the other conditions were the same as those in Example 4.

[0059] The inventors used different amounts of substances in different embodiments and comparative examples, first mechanically stirred and mixed the curing agent and low liquid limit clay evenly, then added water, and mixed evenly again; then sealed with plastic wrap, stored for 12 hours, and then used a compression mold-demolding integrated machine to make a sample with a length of 100 mm and a diameter of 50 mm, and then carried out unconfined compressive strength, direct shear, shrinkage and expansion test specimens, and tested them. The specific process is as follows.

[0060] 1. Unconfined compressive strength test

[0061] The test process was carried out using an unconfined compression apparatus model YAW-300D / 10D.

[0062] How to do it:

[0063] (1) Sample preparation: The material that has been simmered for 12 h is made into a sample with a length of 100 mm and a diameter of 50 mm using a press-molding and demolding machine, and the height is measured and the weight is weighed;

[0064] (2) Curing: All samples were cured in a standard curing box for 7 days at a temperature of 20 ± 2 °C and a relative humidity of 95 ± 3%.

[0065] (3) Test: The unconfined compressive strength machine parameters were adjusted to a loading speed of 1 mm / min. The procedure was based on the Unconfined Compressive Strength Test for Inorganic Bonded Materials in Highway Engineering [JTG E51-2009]. The test was conducted after the sample surface was scraped flat, the height was measured, and the mass was weighed. The results are shown in Table 2 and Figure 1 , the dosage of pretreated furfural residue in the figure is the weight ratio of pretreated furfural residue to low liquid limit clay.

[0066] 2. Shear test

[0067] In the direct shear test, the solidification quick shear test is adopted and carried out in strict accordance with the requirements of the test regulations. The test process is carried out using a direct shear apparatus with the model ZJ Quadruplex Strain Controllde.

[0068] How to do it:

[0069] (1) Align the upper and lower boxes of the shear container and insert the fixing pins, and place the permeable stone and filter paper into the lower box.

[0070] (2) Align the blade of the ring knife and the sample (specimen with a length of 100 mm and a diameter of 50 mm) upwards to the opening of the shear box, place filter paper and permeable stone on the sample, and carefully push the sample into the shear box for testing.

[0071] (3) The shear displacement and shear stress of the clay samples modified by furfural residue pretreatment with different dosages were obtained, and the shear strength of the modified clay was calculated. The shear strength of the specimens was calculated by the shear strength index cohesion (c) and internal friction angle (φ). The vertical loading was set to 4 horizontal loads of 100, 200, 300, and 400 kN, and the shear rate was about 0.8 mm / min. The shearing of the specimens was controlled to be completed within 3-5 min. The results are shown in Table 2 and Figure 2 , the dosage of pretreated furfural residue in the figure is the weight ratio of pretreated furfural residue to low liquid limit clay.

[0072] 3. Shrinkage test

[0073] The test was carried out using a SS-1 shrinkage instrument.

[0074] How to do it:

[0075] (1) Push the prepared specimen (100 mm in length and 50 mm in diameter) out of the ring cutter and place it on the perforated plate.

[0076] (2) Weigh the mass of the sample and the porous plate, install the dial gauge and record the initial reading. Record the percentage reading every 1-4 hours, and then weigh the weight of the entire device and the sample. After 2 days, record the dial gauge reading every 6-24 hours and weigh the weight of the entire device and the sample until the two percentage readings are consistent. The results are shown in Figure 3 and Table 2, in which the dosage of pretreated furfural residue is the weight ratio of the pretreated furfural residue to the weight of the low liquid limit clay.

[0077] 4. Expansion test

[0078] The test was carried out using a WZ-2 dilatometer.

[0079] How to do it:

[0080] (1) Place a wet permeable stone in the base and screw the blunt end of the ring cutter onto the base so that the surface of the sample contacts the top surface of the permeable stone.

[0081] (2) After the specimen (100 mm in length and 50 mm in diameter) is in place, place the piston plate with holes on the top of the specimen, align it with the center of the piston, install the dial indicator and record the dial indicator reading.

[0082] (3) Pour pure water into the basin and keep the water level in the basin roughly the same as the bottom of the sample.

[0083] (4) Record the time when water injection begins, and record the dial gauge readings at 5, 10, 20, 30 min, 1, 2, 3, 24 h, and every 24 hours thereafter until the sample stops expanding. Figure 4and Table 2, in which the dosage of pretreated furfural residue is the weight ratio of the pretreated furfural residue to the weight of the low liquid limit clay.

[0084] Table 2

[0085]

[0086] Depend on Figure 1-4 As shown in Table 2, the unconfined compressive strength value of the modified clay for roadbed of the present invention increases with the increase of the pre-treated furfural slag content, but when the pre-treated furfural slag content exceeds 15% of the low liquid limit clay, the value of the unconfined compressive strength begins to decrease. When the pre-treated furfural slag content reaches more than 20% of the low liquid limit clay, the pre-treated furfural slag content is too high, and the standard sample cannot be supported by the mold-demolding integrated machine for testing. It is worth noting that when the pre-treated furfural slag content is 15% of the low liquid limit clay, the unconfined compressive strength value is the largest, reaching 876.14 kPa after curing for 7 days, exceeding the modified clay prepared with lime as a curing agent (Comparative Example 4), and 532.47 kPa higher than the unconfined compressive strength value of the low liquid limit clay (343.67 kPa).

[0087] With the increase of the pretreated furfural residue content, the cohesion and internal friction angle of the pretreated furfural residue modified clay gradually increased, but when the pretreated furfural residue content exceeded 15% of the low liquid limit clay, the cohesion and internal friction angle showed a slow downward trend. When the pretreated furfural residue content was 15% of the low liquid limit clay, the cohesion and internal friction angle of the clay were the highest, which were 247.4% and 31.5% higher than the low liquid limit clay, respectively, and the shear strength was excellently improved.

[0088] As the amount of pretreated furfural residue increases, the linear shrinkage (es) and volume shrinkage (ev) gradually decrease, but when the amount of pretreated furfural residue exceeds 15% of the low liquid limit clay, the linear shrinkage (es) and volume shrinkage (ev) begin to increase. When the amount of pretreated furfural residue reaches 15% of the low liquid limit clay and reaches the minimum value, the linear shrinkage (es) and volume shrinkage (ev) are reduced by 16.7% and 37.1% respectively compared with comparative example 1, and the anti-shrinkage performance is significantly improved.

[0089] The no-load expansion rate of comparative example 1 is 10.1%. When the dosage of pretreated furfural slag increases from 0% to 15% of low liquid limit clay, the expansion rate of clay decreases significantly, by 40.6%. When the dosage increases from 15% to 18% of low liquid limit clay, the expansion rate of clay begins to rebound and no longer decreases, but is lower than that of blank clay. When the dosage of pretreated furfural slag is 15% of low liquid limit clay, the minimum expansion rate is 6.00%. It can be seen that pretreated furfural slag has an improvement effect on the expansion rate of low liquid limit clay. When the dosage of pretreated furfural slag reaches a certain level, the improvement effect on clay is not obvious. When the dosage of pretreated furfural slag is 15% of low liquid limit clay, the inhibition effect on the expansion performance of low liquid limit clay is the best.

[0090] The performance of the modified clay prepared by using pure cellulose or lignin as a curing agent is lower than that of the examples of the present invention.

[0091] The inventors also optimized the curing agent, and selected a mixture of phosphoric acid aqueous solution and pretreated furfural residue in a mass ratio of 1:1-3 as the curing agent, and the obtained modified clay had better performance. The details are as follows.

[0092] A modified clay for roadbed is composed of the following components in parts by weight: 100 parts by weight of low liquid limit clay; 6-18 parts by weight of pretreated furfural slag; 2-15 parts by weight of phosphoric acid aqueous solution; 7.5-19.2 parts by weight of water; wherein the mass ratio of the phosphoric acid aqueous solution to the pretreated furfural slag is 1:1-3; the concentration of the phosphoric acid aqueous solution is 10wt%, and the total moisture content of the modified clay for roadbed is 21 parts by weight, that is, the total weight of the water in the phosphoric acid aqueous solution and the added water is 21 parts by weight. Specific embodiments are as follows.

[0093] Example 7

[0094] A modified clay for roadbed is composed of the following components by weight: 100 parts by weight of low liquid limit clay; 6 parts by weight of pretreated furfural residue; 6 parts by weight of phosphoric acid aqueous solution; and 15.4 parts by weight of water. The rest is the same as in Example 1.

[0095] Embodiment 8-14

[0096] The substances and amounts of modified clay for roadbed in Examples 8-14 are shown in Table 3, and the other conditions are the same as in Example 7.

[0097] In order to further illustrate the beneficial effects of the present invention, the following comparative example was constructed.

[0098] Comparative Example 7

[0099] The amounts of the substances used in Comparative Example 7 are shown in Table 3, and the other conditions are the same as those in Example 7.

[0100] Table 3

[0101]

[0102] The inventors tested the unconfined compressive strength, direct shear, shrinkage and expansion properties of the modified clay prepared in the above examples and comparative examples. The results are as follows: Figure 5 and Table 4 below.

[0103] Table 4

[0104]

[0105] As can be seen from Table 4, when the curing agent is a mixture of phosphoric acid aqueous solution and pretreated furfural slag, the unconfined compressive strength of the prepared modified clay for roadbed is much higher than that of Examples 1-6, and the unconfined compressive strength of the modified clay for roadbed in Examples 10-13 is also higher than that of the modified clay when cement is used as the curing agent. When the amount of phosphoric acid is large (Comparative Example 7), the moisture content of the prepared sample is too high and cannot meet the test requirements.

[0106] The inventors also simply washed and dried the purchased furfural residue to obtain purified furfural residue, which was used as a curing agent. The performance of the obtained modified clay was better than that of the pre-treated furfural residue in Examples 1-6. The details are as follows.

[0107] A modified clay for roadbed is composed of the following components in parts by weight: 100 parts by weight of low liquid limit clay; 3-20 parts by weight of purified furfural residue; and 21 parts by weight of water. Specific embodiments are as follows.

[0108] Embodiment 15

[0109] A modified clay for roadbed, comprising the following components by weight: 100 parts by weight of low liquid limit clay; 3 parts by weight of purified furfural residue; 21 parts by weight of water;

[0110] The purified furfural residue is obtained by the following steps:

[0111] 1) Place the purchased furfural residue into a double-layer filter bag and rinse with water at a flow rate of about 0.8 m / s for 12 hours;

[0112] 2) drying the washed furfural residue in an oven at 105°C;

[0113] 3) The dried furfural residue is sieved through a sieve with a pore size of 0.5 mm to obtain purified furfural residue;

[0114] The modified clay for roadbed is prepared by the following method: firstly, the low liquid limit clay and the curing agent are mechanically stirred and mixed evenly, and then water is added and stirred evenly.

[0115] Examples 16-21

[0116] The substances and amounts of modified clay for roadbed in Examples 16-21 are shown in Table 5, and the other conditions are the same as in Example 15.

[0117] Table 5

[0118]

[0119] The inventors conducted unconfined compressive strength, direct shear, shrinkage and expansion performance tests on the modified clay prepared in the above examples. The results are shown in Table 6 below.

[0120] Table 6

[0121]

[0122] It can be seen from Table 6 that the performance of the modified clay prepared by using furfural residue after water washing and drying as a curing agent is better than that of Examples 1-6.

[0123] The inventors used purified furfural residue and phosphoric acid aqueous solution as curing agents, and the obtained modified clay also had good performance. The details are as follows.

[0124] A modified clay for roadbed, composed of the following components by weight: 100 parts by weight of low liquid limit clay; 3-18 parts by weight of purified furfural slag; 2-15 parts by weight of phosphoric acid aqueous solution; 7.5-19.2 parts by weight of water; the mass ratio of the phosphoric acid aqueous solution to the purified furfural slag is 1:1-3; the concentration of the phosphoric acid aqueous solution is 10wt%; the total moisture content of the modified clay for roadbed is 21 parts by weight, that is, the total weight of the water in the phosphoric acid aqueous solution and the added water is 21 parts by weight. Specific embodiments are as follows.

[0125] Embodiment 22

[0126] A modified clay for roadbed is composed of the following components in parts by weight: 100 parts by weight of low liquid limit clay; 3 parts by weight of purified furfural residue; 3 parts by weight of phosphoric acid aqueous solution; and 18.3 parts by weight of water. The rest is the same as in Example 15.

[0127] Examples 23-29

[0128] The substances and amounts of modified clay for roadbed in Examples 23-29 are shown in Table 7, and the other conditions are the same as in Example 15.

[0129] In order to further illustrate the beneficial effects of the present invention, the following comparative example was constructed.

[0130] Comparative Example 8

[0131] The amounts of each substance used in Comparative Example 8 are shown in Table 7, and the other conditions are the same as those in Example 22.

[0132] Table 7

[0133]

[0134] The inventors conducted unconfined compressive strength, direct shear, shrinkage and expansion performance tests on the modified clay prepared in the above examples and comparative examples. The results are shown in Table 8.

[0135] Table 8

[0136]

[0137] It can be seen from Table 8 that the performance of the modified clay prepared by purifying furfural residue and phosphoric acid aqueous solution as a curing agent is better than that of Examples 1 to 6. When the amount of phosphoric acid used is large (Comparative Example 8), the moisture content of the prepared sample is too high and cannot meet the test requirements.

[0138] In order to illustrate the influence of the preparation process of purified furfural residue on modified clay, the following example was constructed.

[0139] Embodiment 30

[0140] In this embodiment, the drying temperature during the preparation of purified furfural residue is 150° C., and the other conditions are the same as in Example 15.

[0141] Embodiment 31

[0142] In this embodiment, the drying temperature during the preparation of purified furfural residue is 200° C., and the other conditions are the same as in Example 15.

[0143] Embodiment 32

[0144] In this embodiment, the drying temperature during the preparation of purified furfural residue is 150° C., and the other conditions are the same as in Example 17.

[0145] Embodiment 33

[0146] In this embodiment, the drying temperature during the preparation of purified furfural residue is 200° C., and the other conditions are the same as in Example 17.

[0147] Embodiment 34

[0148] In this embodiment, the drying temperature during the preparation of purified furfural residue is 150° C., and the other conditions are the same as in Example 19.

[0149] Embodiment 35

[0150] In this embodiment, the drying temperature during the preparation of purified furfural residue is 200° C., and the other conditions are the same as in Example 19.

[0151] Embodiment 36

[0152] In this embodiment, the drying temperature during the preparation of purified furfural residue is 80°C, and the other conditions are the same as in Example 19.

[0153] The inventors conducted unconfined compressive strength tests (such as Figure 6 ), direct shear, shrinkage and expansion performance tests, the results are shown in Table 9.

[0154] Table 9

[0155]

[0156] It can be seen from Table 9 that the purified furfural residue obtained at different treatment temperatures has different effects as a curing agent. If the temperature is too low, the drying time will be long and the efficiency will be too low. If the temperature is too high (for example, 250°C), the furfural residue will spontaneously combust and subsequent operations will be impossible.

[0157] When purified furfural residue and phosphoric acid aqueous solution are used as curing agents and the drying temperature is within the range of 80-200°C, the prepared modified clay for roadbed still has good performance, which will not be described in detail here.

[0158] The present invention also provides an application of the modified clay for roadbed, which can be used as highway base or subbase of different grades according to the unconfined compressive strength of the prepared modified clay. The reference is the provisions of 4.2.6 of the "Technical Specifications for Highway Pavement Base Construction" (JTG / T F20-2015).

[0159] In summary, the present invention can greatly improve the unconfined strength, shear strength, shrinkage resistance and expansion resistance of low liquid limit clay by selecting pretreated furfural residue, purified furfural residue or a mixture with phosphoric acid as a curing agent.

[0160] The above is a preferred embodiment of the present invention. For ordinary technicians in this technical field, making several improvements and modifications without departing from the principles of the present invention should also be regarded as within the protection scope of the present invention.

Claims

1. A modified clay for roadbed, characterized in that: The modified clay for roadbed is composed of the following components by weight: 100 parts by weight of low liquid limit clay; 6-20 parts by weight of pretreated furfural residue; 21 parts by weight of water; The pretreated furfural residue is prepared by the following method: the purchased furfural residue is crushed, passed through a 0.5 mm sieve, and then dried in an oven to constant weight, and then sieved through a sieve with an aperture of 0.5 mm to obtain the pretreated furfural residue.

2. A modified clay for roadbed, characterized in that: The modified clay for roadbed is composed of the following components by weight: 100 parts by weight of low liquid limit clay; 6-18 parts by weight of pretreated furfural residue; 2-15 parts by weight of phosphoric acid aqueous solution; 7.5-19.2 parts by weight of water; wherein the mass ratio of the phosphoric acid aqueous solution to the pretreated furfural residue is 1:1-3; the concentration of the phosphoric acid aqueous solution is 10wt%; The total moisture content of the modified clay for roadbed is 21 parts by weight; The pretreated furfural residue is prepared by the following method: the purchased furfural residue is crushed, passed through a 0.5 mm sieve, and then dried in an oven to constant weight, and then sieved through a sieve with an aperture of 0.5 mm to obtain the pretreated furfural residue.

3. A modified clay for roadbed, characterized in that: The modified clay for roadbed is composed of the following components by weight: 100 parts by weight of low liquid limit clay; 3-20 parts by weight of purified furfural residue; 21 parts by weight of water; The purified furfural residue is obtained by the following steps: 1) Place the purchased furfural residue into a filter bag and rinse with water; 2) drying the washed furfural residue in an oven at a temperature of 80-200°C; 3) The dried furfural residue is sieved using a sieve with a pore size of 0.5 mm to obtain purified furfural residue.

4. A modified clay for roadbed, characterized in that: The modified clay for roadbed is composed of the following components by weight: 100 parts by weight of low liquid limit clay; 3-18 parts by weight of purified furfural residue; 2-15 parts by weight of phosphoric acid aqueous solution; 7.5-19.2 parts by weight of water; the mass ratio of the phosphoric acid aqueous solution to the purified furfural residue is 1:1-3; the concentration of the phosphoric acid aqueous solution is 10wt%; The total moisture content of the modified clay for roadbed is 21 parts by weight; The purified furfural residue is obtained by the following steps: 1) Place the purchased furfural residue into a filter bag and rinse with water; 2) drying the washed furfural residue in an oven at a temperature of 80-200°C; 3) The dried furfural residue is sieved using a sieve with a pore size of 0.5 mm to obtain purified furfural residue.

5. The method for preparing modified clay for roadbed according to any one of claims 1 to 4, characterized in that: First, mechanically stir and mix the components except water evenly, then add water and stir again.

6. The use of modified clay for roadbed according to any one of claims 1 to 4, characterized in that: The unconfined compressive strength of the prepared roadbed modified clay is used as the subbase or base of the highway.

Citation Information

Patent Citations

  • Mountain flour curing agent and preparation method thereof

    CN106431160A

  • Low-liquid-limit floury soil composite improved roadbed material and preparation method thereof

    CN108358529A

  • Seasonal frozen soil region subgrade structure and construction method thereof

    CN110184872A