A method for preparing a reverse osmosis membrane modified by POSS structure
The method enhances reverse osmosis membrane flux and desalination efficiency by using amino-modified inorganic particles and cage-type oligomeric silsesquioxane in an interfacial polymerization process, addressing agglomeration issues and improving doping efficiency.
Patent Information
- Application Number
- CN202410918212.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-07-10
AI Technical Summary
Existing reverse osmosis membranes face issues with agglomeration of inorganic particles during doping, leading to reduced membrane flux and desalination efficiency, particularly when using high molar ratios of octaethylene POSS structure with trimesoyl chloride.
A method involving the use of amino-modified inorganic particles and cage-type oligomeric silsesquioxane in an aqueous and oil phase solution, followed by interfacial polymerization on a porous support, to enhance membrane flux by increasing the doping amount and avoiding entanglement of POSS structures.
The method significantly improves membrane flux and desalination efficiency, achieving water fluxes up to 70.2 L·m⁻²·h⁻¹ and retention rates of 99.1% under optimized conditions.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of membrane material preparation for water treatment, and in particular to a modification technology of a reverse osmosis membrane made of polyamide material. Background Art
[0002] Reverse osmosis technology is one of the high-tech industries of the century. Compared with other separation technologies, it has the characteristics of simple operation, no phase change, high efficiency and energy saving, large processing capacity, and high separation efficiency. Reverse osmosis separation technology has been widely used in the fields of seawater and brackish water desalination, wastewater treatment, reclaimed water reuse, food and drug separation. In the entire reverse osmosis technology, reverse osmosis membrane materials are the key core of reverse osmosis technology. Therefore, the preparation of reverse osmosis membrane materials with high performance has always been the hottest research topic in this field.
[0003] To improve membrane flux, it is widely adopted to dope other materials in reverse osmosis membrane, and suitable materials can be inorganic particles, organic small molecules or organic macromolecules with high hydrophilicity. Wherein, inorganic particles include materials such as silicon dioxide, metal organic framework, titanium dioxide and novel carbon nanotubes, graphene, but in the doping process, if the inorganic particles content is too high, agglomeration is likely to occur, thereby limiting the further improvement of membrane flux. To improve this situation, CN107174982A attempts to add octaethylene POSS structure to replace nano silicon dioxide in oil phase solution, thereby avoiding the problems such as agglomeration of inorganic particles. But the actual situation is that when the molar ratio of octaethylene POSS to trimesoyl chloride exceeds 1: 200, the film-forming property of polyamide reverse osmosis composite membrane deteriorates, and there is a bad result of low water flux and desalination rate. Therefore, how to improve the flux of the reverse osmosis membrane doped with further improving POSS structure is a problem to be solved. Summary of the invention
[0004] To solve the above problems, the present invention provides a method for preparing an improved POSS structure-modified reverse osmosis membrane, by selecting the POSS structure and doping particles with an aqueous solution, thereby improving the flux of the membrane from different aspects.
[0005] The present invention provides a method for preparing a reverse osmosis membrane of a POSS structure modification, which comprises the following steps:
[0006] (1) dispersing the amino-modified inorganic particles into an aqueous monomer solution containing a polyamine to form a mixed aqueous solution;
[0007] (2) Eight Sulfonyl chloride The base cage type oligomeric silsesquioxane is dispersed in a polyacyl chloride oil phase monomer solution to obtain a mixed oil phase solution;
[0008] (3) The porous support is sequentially immersed in a mixed aqueous solution and a mixed oil solution to form a reverse osmosis membrane by interfacial polymerization.
[0009] Preferably, the inorganic particles are one or more of silicon dioxide, titanium dioxide, carbon nanotubes, and graphene, and the concentration of the inorganic particles in the mixed aqueous solution is 0.01-0.2 wt %.
[0010] Preferably, the polyamine is selected from one or more of piperazine, m-phenylenediamine, p-phenylenediamine, o-phenylenediamine, ethylenediamine, propylenediamine, and hexamethylenediamine, and its concentration in the mixed aqueous phase solution is 0.05-5wt%.
[0011] Preferably, the solvent in the mixed oil phase solution is one of Isopar G oil, n-hexane, n-heptane and cyclohexane.
[0012] Preferably, the polyacyl chloride is selected from one or more of trimesoyl chloride, terephthaloyl chloride, phthaloyl chloride, and cyclopentanetrichloride.
[0013] Preferably, the eight Sulfonyl chloride The molar ratio of the cage-type oligomeric silsesquioxane to the polyacid chloride is 1:20-1:200.
[0014] Preferably, the porous support is an ultrafiltration or microfiltration membrane selected from one of polyacrylonitrile, polysulfone, polyether, polyethylene, and polyvinylidene fluoride.
[0015] Preferably, the porous support is immersed in the mixed aqueous solution for 20-120 seconds, and in contact with the mixed oil solution for 10-100 seconds.
[0016] The present invention also provides a POSS structure-modified reverse osmosis membrane prepared by the above method, wherein the reverse osmosis membrane contains amino-modified inorganic particles and octahedral Sulfonyl chloride Cage-type oligomeric silsesquioxane.
[0017] First, compared with the prior art, the present invention has the following advantages:
[0018] (1) Through eight Sulfonyl chloride The cage-type oligomeric silsesquioxane as the POSS structure increases the doping amount of the POSS structure, thereby increasing the flux of the membrane.
[0019] (2) By doping inorganic particles in the aqueous phase, the doped inorganic particles will be deposited on the surface of the support after interfacial polymerization, thereby further improving the flux of the membrane.
[0020] (3) The amino groups of the inorganic particles deposited on the surface of the support are combined with the sulfonyl chloride groups of the POSS structure, thereby stretching the POSS macromolecular structure and avoiding the mutual entanglement between the POSS structures, thereby increasing the doping amount of the POSS structure. DETAILED DESCRIPTION
[0021] Example 1
[0022] This embodiment adopts the following method to prepare reverse osmosis membrane:
[0023] (1) dispersing amino-modified nano-silica into a solution containing m-phenylenediamine to form a mixed aqueous phase solution, wherein the m-phenylenediamine concentration in the mixed aqueous phase solution is 2wt% and the nano-silica concentration is 0.1wt%;
[0024] (2) Eight Sulfonyl chloride The base cage type oligomeric silsesquioxane is dispersed into the oil phase monomer solution of trimesoyl chloride to obtain a mixed oil phase solution, wherein the mixed oil phase solution uses cyclohexane as a solvent, wherein the concentration of trimesoyl chloride is 0.2wt%, Sulfonyl chlorine The molar ratio of the cage-type oligomeric silsesquioxane to the polyacid chloride is 1:30;
[0025] (3) The polyethersulfone ultrafiltration membrane is used as a porous support and is first immersed in a mixed aqueous solution for 100 seconds, and then immersed in a mixed oil solution for 60 seconds. Finally, the membrane is picked up and dried to form a reverse osmosis membrane.
[0026] The reverse osmosis membrane was placed under the test conditions of 25°C, 200 psi pressure, and 2000 ppm sodium chloride aqueous solution. After the reverse osmosis membrane was stably operated for 30 minutes, the water flux and desalination rate of the membrane were measured. The results showed that the water flux was 70.2 (L·m -2 ·h -1 ), with a retention rate of 99.1%.
[0027] Example 2
[0028] This embodiment adopts the following method to prepare reverse osmosis membrane:
[0029] (1) dispersing amino-modified nano-silica into a solution containing m-phenylenediamine to form a mixed aqueous phase solution, wherein the m-phenylenediamine concentration in the mixed aqueous phase solution is 2wt% and the nano-silica concentration is 0.1wt%;
[0030] (2) Eight Sulfonyl chloride The base cage type oligomeric silsesquioxane is dispersed into the oil phase monomer solution of trimesoyl chloride to obtain a mixed oil phase solution, wherein the mixed oil phase solution uses cyclohexane as a solvent, wherein the concentration of trimesoyl chloride is 0.2wt%, Sulfonyl chlorine The molar ratio of the cage-type oligomeric silsesquioxane to the polyacid chloride is 1:500;
[0031] (3) The polyethersulfone ultrafiltration membrane is used as a porous support and is first immersed in a mixed aqueous solution for 100 seconds, and then immersed in a mixed oil solution for 60 seconds. Finally, the membrane is picked up and dried to form a reverse osmosis membrane.
[0032] The reverse osmosis membrane was placed under the test conditions of 25°C, 200 psi pressure, and 2000 ppm sodium chloride aqueous solution. After the reverse osmosis membrane was stably operated for 30 minutes, the water flux and desalination rate of the membrane were measured. The results showed that the water flux was 51.7 (L·m -2 ·h -1 ), with a retention rate of 98.2%.
[0033] Comparative Example 1
[0034] This comparative example adopts the following method to prepare reverse osmosis membrane:
[0035] (1) preparing an aqueous solution containing m-phenylenediamine, wherein the concentration of m-phenylenediamine is 2 wt %;
[0036] (2) Eight Sulfonyl chloride The base cage type oligomeric silsesquioxane is dispersed into the oil phase monomer solution of trimesoyl chloride to obtain a mixed oil phase solution, wherein the mixed oil phase solution uses cyclohexane as a solvent, wherein the concentration of trimesoyl chloride is 0.2wt%, Sulfonyl chlorine The molar ratio of the cage-type oligomeric silsesquioxane to the polyacid chloride is 1:30;
[0037] (3) The polyethersulfone ultrafiltration membrane is used as a porous support and is first immersed in an aqueous solution for 100 seconds, and then immersed in a mixed oil solution for 60 seconds. Finally, the membrane is picked up and dried to form a reverse osmosis membrane.
[0038] The reverse osmosis membrane was placed under the test conditions of 25°C, 200 psi pressure, and 2000 ppm sodium chloride aqueous solution. After the reverse osmosis membrane was stably operated for 30 minutes, the water flux and desalination rate of the membrane were measured. The results showed that the water flux was 12.1 (L·m -2 ·h -1 ), with a retention rate of 43.5%.
[0039] Comparative Example 2
[0040] This comparative example adopts the following method to prepare reverse osmosis membrane:
[0041] (1) dispersing amino-modified nano-silica into a solution containing m-phenylenediamine to form a mixed aqueous phase solution, wherein the m-phenylenediamine concentration in the mixed aqueous phase solution is 2wt% and the nano-silica concentration is 0.1wt%;
[0042] (2) preparing an oil phase solution containing trimesoyl chloride oil phase monomer, using cyclohexane as solvent, wherein the concentration of trimesoyl chloride is 0.2 wt %;
[0043] (3) The polyethersulfone ultrafiltration membrane is used as a porous support and is first immersed in the mixed aqueous solution for 100 seconds, and then immersed in the oil phase solution for 60 seconds. Finally, the membrane is picked up and dried to form a reverse osmosis membrane.
[0044] The reverse osmosis membrane was placed under the test conditions of 25°C, 200 psi pressure, and 2000 ppm sodium chloride aqueous solution. After the reverse osmosis membrane was stably operated for 30 minutes, the water flux and desalination rate of the membrane were measured. The results showed that the water flux was 31.2 (L·m -2 ·h -1 ), with a retention rate of 97.0%.
[0045] Comparative Example 3
[0046] This comparative example adopts the following method to prepare reverse osmosis membrane:
[0047] (1) dispersing unmodified nano-silica into a solution containing m-phenylenediamine to form a mixed aqueous phase solution, wherein the m-phenylenediamine concentration of the mixed aqueous phase solution is 2wt% and the nano-silica concentration is 0.1wt%;
[0048] (2) Dispersing octavinyl cage-type oligomeric silsesquioxane into a trimesoyl chloride oil phase monomer solution to obtain a mixed oil phase solution, wherein the mixed oil phase solution uses cyclohexane as a solvent, wherein the concentration of trimesoyl chloride is 0.2 wt %, and the concentration of octavinyl cage-type oligomeric silsesquioxane is 0.2 wt %. Sulfonyl chlorine The molar ratio of the cage-type oligomeric silsesquioxane to the polyacid chloride is 1:30;
[0049] (3) The polyethersulfone ultrafiltration membrane is used as a porous support and is first immersed in a mixed aqueous solution for 100 seconds, and then immersed in a mixed oil solution for 60 seconds. Finally, the membrane is picked up and dried to form a reverse osmosis membrane.
[0050] The reverse osmosis membrane was placed under the test conditions of 25°C, 200 psi pressure, and 2000 ppm sodium chloride aqueous solution. After the reverse osmosis membrane was stably operated for 30 minutes, the water flux and desalination rate of the membrane were measured. The results showed that the water flux was 13.6 (L·m -2 ·h -1), the interception rate is 36.1%. The above-disclosed technical features are not limited to the disclosed combinations with other features, and those skilled in the art can also make other combinations between the technical features according to the purpose of the invention to achieve the purpose of the invention.
Claims
1. A method for preparing a reverse osmosis membrane modified with a POSS structure, Features The steps include: (1) dispersing the amino-modified inorganic particles into an aqueous monomer solution containing a polyamine to form a mixed aqueous solution; (2) Eight Sulfonyl chloride The base cage type oligomeric silsesquioxane is dispersed in a polyacyl chloride oil phase monomer solution to obtain a mixed oil phase solution; (3) The porous support is sequentially immersed in a mixed aqueous solution and a mixed oil solution to form a reverse osmosis membrane by interfacial polymerization.
2. The method according to claim 1, Features The inorganic particles are one or more of silicon dioxide, titanium dioxide, carbon nanotubes, and graphene, and the concentration of the inorganic particles in the mixed aqueous solution is 0.01-0.2 wt %.
3. The method according to claim 1, Features The polyamine is selected from one or more of piperazine, m-phenylenediamine, p-phenylenediamine, o-phenylenediamine, ethylenediamine, propylenediamine, and hexamethylenediamine, and its concentration in the mixed aqueous phase solution is 0.05-5wt%.
4. The method according to claim 1, Features The solvent in the mixed oil phase solution is one of Isopar G oil, n-hexane, n-heptane and cyclohexane.
5. The method according to claim 1, Features The polyacyl chloride is selected from one or more of trimesoyl chloride, terephthaloyl chloride, phthaloyl chloride, and cyclopentanetrichloride, and its concentration in the mixed oil phase solution is 0.02-0.5wt%.
6. The method according to claim 1, Features The eight Sulfonyl chloride The molar ratio of the cage-type oligomeric silsesquioxane to the polyacid chloride is 1:20-1:
200.
7. The method according to claim 1, Features The porous support is an ultrafiltration or microfiltration membrane, selected from one of polyacrylonitrile, polysulfone, polyether, polyethylene, and polyvinylidene fluoride.
8. The method according to claim 1, Features The porous support body is immersed in the mixed water phase solution for 20-120 seconds, and is in contact with the mixed oil phase solution for 10-100 seconds.
9. A reverse osmosis membrane with modified POSS structure prepared according to the method of claim 1, Features The reverse osmosis membrane contains amino-modified inorganic particles and eight Sulfonyl chloride Cage-type oligomeric silsesquioxane.