Super high early strength shotcrete admixture and preparation method and application thereof

By preparing an ultra-high early strength shotcrete admixture, the problem of insufficient early strength of shotcrete has been solved, and the early strength and later strength have been significantly improved. It is suitable for various construction environments and is applicable to projects such as mining, water conservancy and tunnels.

CN118637855BActive Publication Date: 2024-11-19四川昊龙高科轨道交通新材料科技股份有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411106207.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-19
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

Existing shotcrete has a slow early strength development, which makes it impossible to seal and reinforce the surrounding rock in time, leading to structural settlement, deformation and crack formation. In addition, nanomaterials are prone to agglomeration, affecting the later strength. There is a lack of efficient and low-dosage early strength agents.

Method used

The ultra-high early strength shotcrete admixture is composed of silica fume, water-reducing agent, crystal nucleation early strength agent, modified ester, suspending agent, sodium carbonate and polyvinyl alcohol fiber. It is prepared by controlling the temperature and stirring process to improve early strength and maintain later strength. It is easy to use and adaptable to various construction environments.

Benefits of technology

It significantly improves the early strength of shotcrete and doubles its later strength, making it suitable for projects such as mining, water conservancy, and tunnels. It also reduces dust, adapts to various construction environments, and improves the pumpability and workability of shotcrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 42JJLV6QLWSAUOZCLCFJHNQDSZC8DEPGBBTDXU5P
    Figure 42JJLV6QLWSAUOZCLCFJHNQDSZC8DEPGBBTDXU5P
  • Figure 6W7WU1ZZBMIWLO8ZQWZSNL23UOKQI8EYGRISBFOO
    Figure 6W7WU1ZZBMIWLO8ZQWZSNL23UOKQI8EYGRISBFOO
  • Figure DVRPBSHNFI6QCAH7HNWPF3M12OATL8RTDZQJQ4YH
    Figure DVRPBSHNFI6QCAH7HNWPF3M12OATL8RTDZQJQ4YH
Patent Text Reader

Abstract

The present invention relates to the technical field of building materials, specifically to an ultra-high early strength shotcrete admixture and a preparation method and application thereof, wherein the admixture comprises the following components: silica fume, a water reducing agent, a crystal nucleus early strength agent, a modified ester, acrylic acid, a suspending agent, sodium carbonate, polyvinyl alcohol fiber and water. The ultra-high early strength shotcrete admixture of the present invention is an aqueous solution, which is convenient to use, reduces dust, has good pumpability, and can adapt to a variety of construction environments. In addition, the admixture has a low dosage, can significantly improve the early strength of shotcrete, and improves the final strength. It is suitable for the prevention and control of rock bursts in mines, water conservancy, tunnels, and subways, and the spraying of seepage tunnel sections, which can solve the spraying process that conventional shotcrete cannot complete in seepage tunnel sections.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, in particular to an ultra-high early strength shotcrete admixture and a preparation method and application thereof. Background Art

[0002] Shotcrete is a kind of support structure material. It is sprayed on the rock surface by mechanical arms with quick-setting agent. It can quickly solidify into a layer of support structure, thus supporting the rock layer and protecting the subsequent work. The most common silicate shotcrete has a slow early strength growth rate and cannot really play its role of timeliness, sealing and bonding. Because for tunnels in weak, loose and broken strata, a process cycle is often kept within 24 hours, which means that the next blasting operation needs to be carried out within 0.5 to 4 hours after the shotcrete spraying is completed. At this time, if the strength of the shotcrete is insufficient, it will not only fail to seal and reinforce the surrounding rock in time, but also increase the deadweight of the structure. Under the action of blasting vibration, construction disturbance additional load and deadweight of the structure, the initial support structure settles and deforms, and is separated from the surrounding rock behind to form cracks or cavities, which then induces the traction relaxation of the surrounding rock, bringing difficulties to the surrounding rock support. The 4h strength of ordinary silicate shotcrete is only 0.86MPa, and the 24h strength is only 11.8MPa. The development of early strength of shotcrete plays a decisive role in support and has a direct impact on the excavation progress. The early strength of shotcrete is more important than the final strength.

[0003] Crystal nucleus early strength agent is a new type of early strength agent that can provide the crystal nuclei required for early hydration of cement and promote the precipitation of hydration products. With the widespread application of nanomaterials, it is easy to cause nanoparticles to agglomerate and precipitate, and cannot exist stably for a long time, which brings certain difficulties to the application of crystal nucleus early strength agent. Moreover, since it can only improve the early strength, the effect of improving the later strength is not obvious.

[0004] In summary, there is an urgent need for a concrete admixture that has high early strength, low dosage, is easy to use, has high later strength, and is suitable for shotcrete. Summary of the invention

[0005] The purpose of the present invention is to overcome the deficiencies of the prior art and to provide an ultra-high early strength shotcrete admixture and a preparation method and application thereof, so as to at least achieve the effect of effectively improving the early strength of concrete with a low dosage.

[0006] The objective of the present invention is achieved through the following technical solutions:

[0007] A super-high early-strength shotcrete admixture comprises the following components: silica fume, a water reducing agent, a crystal nucleus early-strengthening agent, a modified ester, acrylic acid, a suspending agent, sodium carbonate, polyvinyl alcohol fiber and water.

[0008] Furthermore, the components include, by weight: 190 parts of silica fume, 90-120 parts of water reducing agent, 350-500 parts of crystal nucleus early strength agent, 53 parts of modified ester, 10 parts of acrylic acid, 0.15-0.6 parts of suspending agent, 5.5 parts of sodium carbonate, 4 parts of polyvinyl alcohol fiber and 152-438 parts of water.

[0009] Furthermore, the particle size of the silica fume is 0.01 to 0.5 µm.

[0010] Furthermore, the preparation method of the modified ester is: grafting a carboxylic acid polymer with a molecular weight of 1000-2000 with polyethylene oxide having an alkoxy group at one end and a hydroxyl group or an amino group at the other end in a non-aqueous solvent; or modifying with a polyene polyamine polymer, selecting a carboxylic acid polymer having a molecular weight of 1000-2000 and a polyoxyethylene having an alkoxy group at one end and a hydroxyl group or an amino group at the other end; 3- Acrylic acid, 2-acrylamide-2-methylpropanesulfonic acid and polyethylene glycol monoacrylate containing non-polar groups -OH and -CH2CH20- are used as reaction monomers, which are grafted onto molecules containing NH2 through Michael addition in aqueous solution to obtain the obtained product.

[0011] Furthermore, the modified ester includes at least one of hydroxyethyl ester, hydroxypropyl ester, polyacrylamide, AMPS (2-acrylamide-2-methylpropane sulfonic acid) and phosphate coupling agent.

[0012] Furthermore, the suspending agent is a sodium polyacrylate suspending agent;

[0013] It is worth noting that sodium polyacrylate is commonly used in food suspensions. Sodium polyacrylate can change the electrical properties of the particle surface, thereby reducing the interaction force between particles, avoiding agglomeration and precipitation between particles, and is beneficial to slurry stability.

[0014] Furthermore, the crystal nucleus early strength agent is a calcium silicate hydrate crystal nucleus early strength agent;

[0015] Preferably, the calcium silicate crystal nucleus early strength agent is S7000 liquid crystal seed early strength agent.

[0016] Furthermore, the water reducing agent includes at least one of methyl methacrylate and polyoxyethylene ether.

[0017] Furthermore, the preparation method of the admixture comprises the following steps:

[0018] S1: at 54-56°C, the water reducing agent and the crystal nucleus early strength agent are mixed and stirred evenly, and then the silica fume is added, and the temperature is raised to 72-78°C and stirred;

[0019] S2: adding the material obtained in step S1 to the modified ester, the acrylic acid and water, and stirring;

[0020] S3: adding the material obtained in step S2 to the suspending agent and stirring;

[0021] S4: adding the material obtained in step S3 to the sodium carbonate, the polyvinyl alcohol fiber and water, and maintaining the temperature above 95° C. to obtain the concrete admixture.

[0022] It is worth noting that the components in the admixture of the present invention need to be added under controlled temperature, otherwise it will lead to the loss of some components and the effect will be deteriorated.

[0023] Furthermore, the method for using the admixture includes: adding the admixture to the cementitious material in an amount of 3%-6%.

[0024] Furthermore, the method of use also includes: directly mixing the admixture with the gelling material.

[0025] Furthermore, the admixture is used for shotcrete support.

[0026] It is worth noting that: the crystal nucleus early strength agent can promote the early cement hydration process and improve the early strength of concrete, but does not affect the final strength; the suspending agent pre-disperses the high-activity mineral powder before encapsulating it, so that the high-activity mineral after slow release can obtain sufficient reaction area, thereby accelerating the strength development rate of concrete; polyvinyl alcohol fiber can improve the tensile, bending, frost and fatigue resistance of concrete; the role of sodium carbonate is to adjust the pH; the role of sodium carbonate is to adjust the pH; the water reducer can reduce the amount of mixing water while maintaining the slump of concrete unchanged, improve its workability, increase the strength of concrete and improve durability; modified esters and acrylic acid are used as slump retainers to maintain the slump and activity of concrete; the water reducer can avoid the reduction of the working performance of shotcrete and improve pumpability.

[0027] The beneficial effects of the present invention are:

[0028] 1. The dosage of the ultra-high early strength shotcrete admixture of the present invention is 3% to 6% of the mass of the cementitious material, which can significantly improve the early strength of shotcrete. It is suitable for the prevention and control of rock bursts in mines, water conservancy, tunnels, and subways and the spraying of seepage tunnel sections. It can solve the spraying process that conventional shotcrete cannot complete in seepage tunnel sections.

[0029] 2. The admixture of the present invention is an aqueous solution, which is easy to use, reduces dust, has good pumpability, and can adapt to a variety of construction environments.

[0030] 3. The present invention combines the crystal nucleus early strength agent with the suspension agent, which not only has a higher early strength, but also significantly improves the later strength, about doubling the strength. DETAILED DESCRIPTION

[0031] The technical solution of the present invention is further described in detail below, but the protection scope of the present invention is not limited to the following.

[0032] The models and sources of some reagents used in the following examples are as follows:

[0033] Crystal seed early strength agent, model: liquid crystal seed early strength agent S7000, brand: Xinyi Synthesis, specification: 200kg / barrel;

[0034] Suspending agent, sodium polyacrylate, brand: Shandong Qisheng New Materials, specification: 25kg / bag;

[0035] Ultrafine silicon dioxide powder, brand: DeLan Chemical, particle size distribution is mainly 0.01~0.5µm;

[0036] A super high early strength concrete admixture is prepared, and the specific method is as follows:

[0037] 1) Add 50 parts of methyl allyl alcohol, 50 parts of polyoxyethylene ether, 350 parts of early strength crystal nucleating agent and 150 parts of water into a stirring kettle, keep the temperature at 55°C, mix and stir, add 190 parts of ultrafine silicon dioxide powder and 5 parts of emulsifier after 30 minutes, then raise the temperature to 55°C and continue stirring for 90 minutes;

[0038] 2) 53 parts of polyacrylamide, 10 parts of acrylic acid and 10 parts of water were mixed to prepare a solution, added to a reactor, stirred for 90 minutes, and then 0.5 parts of a suspending agent was added and stirred for another 90 minutes;

[0039] 3) 5.5 parts of sodium carbonate, 4 parts of pure polyethylene fiber and 10 parts of water are mixed to prepare a solution, which is added into a reactor and stirred for 90 minutes. During the stirring process, the temperature is controlled to be not less than 95° C. The obtained suspension is the admixture.

[0040] A super high early strength concrete admixture is prepared, and the specific method is as follows:

[0041] 1) Add 60 parts of methyl allyl alcohol, 60 parts of polyoxyethylene ether, 400 parts of early strength crystal nucleating agent and 200 parts of water into a stirring kettle, keep the temperature at 55°C, mix and stir, add 190 parts of ultrafine silicon dioxide powder and 5 parts of emulsifier after 30 minutes, then raise the temperature to 55°C and continue stirring for 90 minutes;

[0042] 2) 53 parts of polyacrylamide, 10 parts of acrylic acid and 10 parts of water were mixed to prepare a solution, added to a reactor, stirred for 90 minutes, and then 0.2 parts of a suspending agent was added and stirred for another 90 minutes;

[0043] 3) 5.5 parts of sodium carbonate, 4 parts of pure polyethylene fiber and 10 parts of water are mixed to prepare a solution, which is added into a reactor and stirred for 90 minutes. During the stirring process, the temperature is controlled to be not less than 95° C. The obtained suspension is the admixture.

[0044] A super high early strength concrete admixture is prepared, and the specific method is as follows:

[0045] 1) Add 80 parts of methyl allyl alcohol, 40 parts of polyoxyethylene ether, 500 parts of early strength crystal nucleating agent and 200 parts of water into a stirring tank, keep the temperature at 55°C, mix and stir, add 190 parts of ultrafine silicon dioxide powder and 5 parts of emulsifier after 30 minutes, then raise the temperature to 55°C and continue stirring for 90 minutes;

[0046] 2) 53 parts of polyacrylamide, 10 parts of acrylic acid and 10 parts of water were mixed to prepare a solution, added to a reactor, stirred for 90 minutes, and then 0.6 parts of a suspending agent was added and stirred for another 90 minutes;

[0047] 3) 5.5 parts of sodium carbonate, 4 parts of pure polyethylene fiber and 10 parts of water are mixed to prepare a solution, which is added into a reactor and stirred for 90 minutes. During the stirring process, the temperature is controlled to be not less than 95° C. The obtained suspension is the admixture.

[0048] A super high early strength concrete admixture is prepared, and the specific method is as follows:

[0049] 1) Add 100 parts of methyl allyl alcohol, 350 parts of early strength crystal nucleating agent and 150 parts of water into a stirring kettle, keep the temperature at 55°C, mix and stir, add 190 parts of ultrafine silicon dioxide powder and 5 parts of emulsifier after 30 minutes, then raise the temperature to 55°C and continue stirring for 90 minutes;

[0050] 2) Mix 53 parts of AMPS, 10 parts of acrylic acid and 10 parts of water to prepare a solution, add it to the reactor, stir for 90 minutes, then add 0.5 parts of suspending agent and continue stirring for 90 minutes;

[0051] 3) 5.5 parts of sodium carbonate, 4 parts of pure polyethylene fiber and 10 parts of water are mixed to prepare a solution, which is added into a reactor and stirred for 90 minutes. During the stirring process, the temperature is controlled to be not less than 95° C. The obtained suspension is the admixture.

[0052] Comparative Example 1

[0053] An ultra-high early strength concrete admixture is prepared, which differs from Example 1 in that no crystal nucleus early strength agent is added, and the specific method is as follows:

[0054] 1) Add 50 parts of methyl allyl alcohol, 50 parts of polyoxyethylene ether and 150 parts of water into a stirring kettle, keep the temperature at 55°C, mix and stir, add 190 parts of ultrafine silicon dioxide powder and 5 parts of emulsifier after 30 minutes, then raise the temperature to 55°C and continue stirring for 90 minutes;

[0055] 2) 53 parts of modified ester, 10 parts of acrylic acid and 10 parts of water were mixed to prepare a solution, added to a reaction kettle, stirred for 90 minutes, and then 0.5 parts of a suspending agent was added and stirred for another 90 minutes;

[0056] 3) 5.5 parts of sodium carbonate, 4 parts of pure polyethylene fiber and 10 parts of water are mixed to prepare a solution, which is added into a reactor and stirred for 90 minutes. During the stirring process, the temperature is controlled to be not less than 95° C. The obtained suspension is the admixture.

[0057] Comparative Example 2

[0058] An ultra-high early strength concrete admixture is prepared, which differs from Example 1 in that no suspending agent is added, and the specific method is as follows:

[0059] 1) Add 50 parts of methyl allyl alcohol, 50 parts of polyoxyethylene ether, 350 parts of early strength crystal nucleating agent and 150 parts of water into a stirring kettle, keep the temperature at 55°C, mix and stir, add 190 parts of ultrafine silicon dioxide powder and 5 parts of emulsifier after 30 minutes, then raise the temperature to 55°C and continue stirring for 90 minutes;

[0060] 2) 53 parts of polyacrylamide, 10 parts of acrylic acid and 10 parts of water were mixed to prepare a solution, added to the reactor and stirred for 90 minutes;

[0061] 3) 5.5 parts of sodium carbonate, 4 parts of pure polyethylene fiber and 10 parts of water are mixed to prepare a solution, which is added into a reactor and stirred for 90 minutes. During the stirring process, the temperature is controlled to be not less than 95° C. The obtained suspension is the admixture.

[0062] Comparative Example 3

[0063] An ultra-high early strength concrete admixture is prepared. The difference from Example 1 is that no crystal nucleus early strength agent and suspending agent are added. The specific method is as follows:

[0064] 1) Add 50 parts of methyl allyl alcohol, 50 parts of polyoxyethylene ether and 300 parts of water into a stirring kettle, keep the temperature at 55°C, mix and stir, add 190 parts of ultrafine silicon dioxide powder and 5 parts of emulsifier after 30 minutes, then raise the temperature to 55°C and continue stirring for 90 minutes;

[0065] 2) 53 parts of polyacrylamide, 10 parts of acrylic acid and 10 parts of water were mixed to prepare a solution, added to the reactor and stirred for 90 minutes;

[0066] 3) 5.5 parts of sodium carbonate, 4 parts of pure polyethylene fiber and 10 parts of water are mixed to prepare a solution, which is added into a reactor and stirred for 90 minutes. During the stirring process, the temperature is controlled to be not less than 95° C. The obtained suspension is the admixture.

[0067] Comparative Example 4

[0068] An ultra-high early strength concrete admixture is prepared. The difference from Example 1 is that a different type of early strength agent is used. The specific method is as follows:

[0069] 1) Add 50 parts of methyl allyl alcohol, 50 parts of polyoxyethylene ether, 350 parts of early strength agent (triethanolamine early strength agent, brand: Jinglong Technology) and 150 parts of water into a stirring kettle, keep the temperature at 55°C, mix and stir, add 190 parts of ultrafine silicon dioxide powder and 5 parts of emulsifier after 30 minutes, then raise the temperature to 55°C and continue stirring for 90 minutes;

[0070] 2) 53 parts of polyacrylamide, 10 parts of acrylic acid and 10 parts of water were mixed to prepare a solution, added to a reactor, stirred for 90 minutes, and then 0.5 parts of a suspending agent was added and stirred for another 90 minutes;

[0071] 3) 5.5 parts of sodium carbonate, 4 parts of pure polyethylene fiber and 10 parts of water are mixed to prepare a solution, which is added into a reactor and stirred for 90 minutes. During the stirring process, the temperature is controlled to be not less than 95° C. The obtained suspension is the admixture.

[0072] Comparative Example 5

[0073] An ultra-high early strength concrete admixture is prepared, which differs from Example 1 in that a different type of suspending agent is used. The specific method is as follows:

[0074] 1) Add 50 parts of methyl allyl alcohol, 50 parts of polyoxyethylene ether, 350 parts of early strength agent and 150 parts of water into a stirring kettle, keep the temperature at 55°C, mix and stir, add 190 parts of ultrafine silicon dioxide powder and 5 parts of emulsifier after 30 minutes, then raise the temperature to 55°C and continue stirring for 90 minutes;

[0075] 2) Mix 53 parts of polyacrylamide, 10 parts of acrylic acid and 10 parts of water to prepare a solution, add it to the reactor, stir for 90 minutes, then add 0.5 parts of XY600 suspension agent (suspension agent XY-600, brand: Xinyi Synthesis, specification: 20kg / bag. The suspension agent is a water-soluble biopolymer with pseudoplastic and shear-thinning rheological properties, which can improve the slurry stability.) Continue stirring for 90 minutes;

[0076] 3) 5.5 parts of sodium carbonate, 4 parts of pure polyethylene fiber and 10 parts of water are mixed to prepare a solution, which is added into a reactor and stirred for 90 minutes. During the stirring process, the temperature is controlled to be not less than 95° C. The obtained suspension is the admixture.

[0077] Experimental Example 1

[0078] Three different proportions of cement, sand, crushed stone, water and the admixture of Example 1 are mixed and mixed in proportion, and then used in conjunction with an accelerator for the implementation of shotcrete. The admixture content accounts for 5% of the total cementitious material (cement) used for concrete, and the specific proportion is shown in Table 1:

[0079] Table 1

[0080]

[0081] Taking the concrete (according to mix ratio 1) with the existing early strength agent (brand: Chentong Environmental Protection) as the control group, the performance of the shotcrete with the ultra-high early strength shotcrete admixture was tested. The test content and test method are as follows, and the test results are shown in Table 2-3:

[0082] For the quick-setting performance test, refer to Q / CR807 2020 "Liquid alkali-free quick-setting agent for tunnel shotcrete", in which the 6h strength of the mortar is ≥1MPa, and the chloride ion content in the liquid alkali-free quick-setting agent is ≤0.05%, and the alkali content is ≤1%.

[0083] For the testing of admixtures for ultra-high early strength shotcrete, refer to the "Concrete Admixtures" GB8076-2008, "Test Methods for Homogeneity of Concrete Admixtures" GB8077-2012 and the viscosity enhancer testing in TB10424-2018 "Railway Concrete Engineering Construction Quality Acceptance Standards".

[0084] Table 2

[0085]

[0086] Table 3

[0087]

[0088] It can be seen that after field tests of shotcrete, its bonding strength can reach more than 3.2MPa, the thickness of one shotcrete can reach 0.5m, and the rebound rate is reduced. The rebound rate of the shotcrete arch can be controlled at about 5%.

[0089] Experimental Example 2

[0090] The admixtures of Examples 1-4 and Comparative Examples 1-3 were taken at a dosage of 5%, mixed evenly with cement, sand, gravel, and water (according to the ratio 1), and then used in conjunction with an accelerator for the implementation of shotcrete. The performance of the shotcrete with the ultra-high early strength shotcrete admixture was tested. The test content and test method were the same as those of Experimental Example 1. The test results are shown in Tables 4-5

[0091] Table 4

[0092]

[0093]

[0094] Table 5

[0095]

[0096] It can be seen from the above experimental data that when the nucleus early strength agent and the suspension agent are added at the same time, the early strength of the concrete is significantly improved, and the later strength is also significantly increased. The addition of the nucleus early strength agent and the suspension agent not only accelerates the rate of increase in early strength but also increases the later strength.

[0097] The above is only a preferred embodiment of the present invention. It should be understood that the present invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art shall not deviate from the spirit and scope of the present invention, and shall be within the scope of protection of the claims attached to the present invention.

Claims

1. A super-high early strength shotcrete admixture, characterized in that: The invention comprises the following components: silica fume, water reducing agent, crystal nucleus early strength agent, modified ester, acrylic acid, suspending agent, sodium carbonate, polyvinyl alcohol fiber and water; The suspending agent is a sodium polyacrylate suspending agent; The crystal nucleus early strength agent is a calcium silicate hydrate crystal nucleus early strength agent; In parts by weight, the components include: 190 parts of silica fume, 90-120 parts of water reducing agent, 350-500 parts of crystal nucleus early strength agent, 53 parts of modified ester, 10 parts of acrylic acid, 0.15-0.6 parts of suspending agent, 5.5 parts of sodium carbonate, 4 parts of polyvinyl alcohol fiber and 152-438 parts of water; The preparation method of the modified ester is: grafting a carboxylic acid polymer with a molecular weight of 1000-2000 with polyethylene oxide having an alkoxy group at one end and a hydroxyl group or an amino group at the other end in a non-aqueous solvent; or modifying with a polyene polyamine polymer, selecting a polyol containing polar groups -COO-, -SO 3- Acrylic acid, 2-acrylamide-2-methylpropanesulfonic acid and polyethylene glycol monoacrylate containing non-polar groups -OH and -CH2CH2O- are used as reactive monomers, which are grafted onto molecules containing NH2 by Michael addition in aqueous solution; The modified ester includes at least one of hydroxyethyl ester, hydroxypropyl ester, polyacrylamide and AMPS; The water reducing agent includes at least one of methyl allyl alcohol and polyoxyethylene ether.

2. The admixture according to claim 1, characterized in that: The particle size of the silica fume is 0.01-0.5 μm.

3. The method for preparing an admixture as claimed in any one of claims 1 to 2, characterized in that: The following steps are involved: S1: at 54-56°C, the water reducing agent and the crystal nucleus early strength agent are mixed and stirred evenly, and then the silica fume is added, and the temperature is raised to 72-78°C and stirred; S2: adding the material obtained in step S1 to the modified ester, the acrylic acid and water, and stirring; S3: adding the material obtained in step S2 to the suspending agent and stirring; S4: adding the material obtained in step S3 to the sodium carbonate, the polyvinyl alcohol fiber and water, and maintaining the temperature above 95° C. to obtain the concrete admixture.

4. The use of an admixture as claimed in any one of claims 1 to 2, characterized in that: include: The admixture is added to the cementitious material in an amount of 3% to 6%.

5. Use of the admixture as described in any one of claims 1-2 in shotcrete support.