Composite electromagnetic absorbing material and preparation method thereof
By doping rare earth elements and other materials into ferrite absorbing materials, combining epoxy resin as a binder, and using ultrasonic dispersion technology to prepare composite electromagnetic absorbing materials, the insufficient performance of existing ferrite absorbing materials is solved. The problem is that more efficient electromagnetic wave absorption and frequency band expansion are achieved.
Patent Information
- Application Number
- CN202411096297.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-12
AI Technical Summary
The absorption rate and temperature resistance, humidity resistance and corrosion resistance of existing ferrite wave absorbing materials in the high frequency band are insufficient, making it difficult to meet the needs of complex engineering applications.
By doping rare earth elements, combining magnetite powder, nickel powder, copper powder, graphite powder, carbon black powder and barium titanate powder, epoxy resin is used as the binder, and composite electromagnetic wave absorbing materials are prepared through ultrasonic dispersion technology. , improve its absorption performance and bandwidth.
It significantly improves the absorption performance and durability of composite electromagnetic wave absorbing materials, meets higher performance requirements, and achieves better electromagnetic wave absorption effect and frequency band expansion.
Smart Images

Figure CN118637857B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electromagnetic wave absorbing materials, and in particular to a composite electromagnetic wave absorbing material and a preparation method thereof. Background Art
[0002] Electromagnetic absorbing materials refer to a type of material that can absorb or significantly reduce the electromagnetic wave energy received on its surface, thereby reducing the interference of electromagnetic waves. In engineering applications, in addition to requiring the absorbing material to have a high absorption rate of electromagnetic waves in a wide frequency band, it is also required to have properties such as light weight, temperature resistance, moisture resistance, and corrosion resistance. Electromagnetic radiation causes direct and indirect harm to the human body through thermal effects, non-thermal effects, and cumulative effects. Studies have confirmed that ferrite absorbing materials have the best performance. It has the characteristics of high absorption frequency band, high absorption rate, and thin matching thickness. The application of this material in electronic equipment can absorb leaked electromagnetic radiation and achieve the purpose of eliminating electromagnetic interference.
[0003] Ferrite absorbing material is ferrite dispersed in a binder of organic polymer material, and some other additives are added at the same time. However, as the demand in the application field increases, the performance requirements for electromagnetic absorbing materials also increase accordingly. How to improve the comprehensive performance of ferrite electromagnetic absorbing materials is also a problem that needs to be solved at present. Therefore, the present invention proposes a composite electromagnetic absorbing material and a preparation method thereof to solve the problems existing in the prior art. Summary of the invention
[0004] In view of the above problems, the purpose of the present invention is to propose a composite electromagnetic absorbing material and a preparation method. The composite electromagnetic absorbing material and the preparation method thereof are obtained by doping rare earth elements and combining a variety of materials to improve the comprehensive performance of the composite electromagnetic absorbing material, which can solve the problems existing in the prior art.
[0005] To achieve the purpose of the present invention, the present invention is implemented through the following technical scheme: a composite electromagnetic absorbing material and a preparation method, comprising the following raw materials in parts by weight: 50 to 60 parts of magnetite powder, 5 to 8 parts of nickel powder, 5 to 8 parts of copper powder, 2 to 4 parts of samarium oxide, 2 to 4 parts of gadolinium oxide, 2 to 4 parts of cerium oxide, 5 to 7 parts of carbon black powder, 8 to 15 parts of graphite powder, 20 to 30 parts of epoxy resin, 5 to 7 parts of barium titanate powder, 1 to 2 parts of antioxidant, 15 to 20 parts of curing agent, 1 to 2 parts of diluent and 1 to 2 parts of leveling agent.
[0006] The further improvement is that the following raw materials are included in weight parts: 60 parts of magnetite powder, 5 parts of nickel powder, 5 parts of copper powder, 2 parts of samarium oxide, 2 parts of gadolinium oxide, 2 parts of cerium oxide, 7 parts of carbon black powder, 8 parts of graphite powder, 20 parts of epoxy resin, 7 parts of barium titanate powder, 2 parts of antioxidant, 15 parts of curing agent, 2 parts of diluent and 2 parts of leveling agent.
[0007] The further improvement is that the following raw materials are included in weight parts: 50 parts of magnetite powder, 8 parts of nickel powder, 8 parts of copper powder, 4 parts of samarium oxide, 4 parts of gadolinium oxide, 4 parts of cerium oxide, 5 parts of carbon black powder, 15 parts of graphite powder, 30 parts of epoxy resin, 5 parts of barium titanate powder, 1 part of antioxidant, 20 parts of curing agent, 1 part of diluent and 1 part of leveling agent.
[0008] A further improvement is that the samarium oxide, gadolinium oxide, cerium oxide and barium titanate powder are all in powder form.
[0009] A further improvement is that the antioxidant is a phenol antioxidant, the curing agent is an aromatic amine curing agent diethyltoluenediamine, the diluent is polyol glycidyl ether, the leveling agent is silicone oil, and the epoxy resin is bisphenol A epoxy resin.
[0010] A method for preparing a composite electromagnetic absorbing material comprises the following steps:
[0011] Step 1: Material preparation
[0012] According to the formula, weigh 50-60 parts of magnetite powder, 5-8 parts of nickel powder, 5-8 parts of copper powder, 2-4 parts of samarium oxide, 2-4 parts of gadolinium oxide, 2-4 parts of cerium oxide, 5-7 parts of carbon black powder, 8-15 parts of graphite powder, 20-30 parts of epoxy resin, 5-7 parts of barium titanate powder, 1-2 parts of antioxidant, 15-20 parts of curing agent, 1-2 parts of diluent and 1-2 parts of leveling agent;
[0013] Step 2: Mixing of absorbing magnetic materials
[0014] The magnetite powder, nickel powder and copper powder are ground by ultrafine powder grinders respectively, and then added into a dry powder mixer, and then graphite powder, carbon black powder and barium titanate powder are added and stirred to obtain a wave absorbing magnetic material;
[0015] Step 3: Mixing of rare earth materials
[0016] The samarium oxide, gadolinium oxide and cerium oxide are dried in a vacuum drying oven, and after drying, they are mixed in a dry powder mixer to obtain a mixed rare earth oxide material;
[0017] Step 4: Preparation of composite electromagnetic absorbing materials
[0018] The epoxy resin and the curing agent are stirred and mixed under a heating environment, and then a diluent is added and stirred continuously to obtain a mixed matrix, and then the absorbing magnetic material in step 2 and the mixed rare earth oxide material in step 3 are added and mixed again. During the mixing process, an antioxidant and a leveling agent are added and mixed for ultrasonic dispersion to obtain a composite electromagnetic absorbing material.
[0019] A further improvement is that in the step 2, the particle sizes of the magnetite powder, nickel powder and copper powder are controlled to be 2-5 μm by using an ultra-fine powder grinder.
[0020] A further improvement is that the drying is vacuum drying with the following parameters: temperature of 90 to 120° C. and drying time of 10 to 20 minutes.
[0021] A further improvement is that in step 4, the heating environment is 60-80°C.
[0022] The beneficial effects of the present invention are as follows: the composite electromagnetic absorbing material provided by the present invention takes the ferrite absorbing material as the matrix, is composited by combining nickel powder, copper powder, graphite powder, carbon black and barium titanate, and then doped with mixed rare earth oxides by combining samarium oxide, gadolinium oxide and cerium oxide, and then on the basis of the above, a composite electromagnetic absorbing material is prepared, which combines the magnetic loss characteristics of magnetite powder, the ferromagnetic behavior of nickel powder and the electrical conductivity of copper powder, which is conducive to achieving good electromagnetic wave absorption performance, and then by introducing graphite powder, carbon black powder and barium titanate powder as fillers to improve the performance of the composite electromagnetic absorbing material, and then by using rare earth doping to improve the wave absorption characteristics of the composite electromagnetic material, the performance of the composite electromagnetic material is comprehensively improved to meet the demand for higher performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a schematic diagram of the steps of the preparation method of the present invention. DETAILED DESCRIPTION
[0024] In order to deepen the understanding of the present invention, the present invention will be further described in detail below in conjunction with examples. The examples are only used to explain the present invention and do not constitute a limitation on the protection scope of the present invention.
[0025] The raw materials used in the following examples were all obtained through conventional commercial routes.
[0026] Embodiment 1
[0027] according to Figure 1 As shown, this embodiment proposes a composite electromagnetic absorbing material, including the following raw materials in parts by weight: 60 parts of magnetite powder, 5 parts of nickel powder, 5 parts of copper powder, 2 parts of samarium oxide, 2 parts of gadolinium oxide, 2 parts of cerium oxide, 7 parts of carbon black powder, 8 parts of graphite powder, 20 parts of epoxy resin, 7 parts of barium titanate powder, 2 parts of antioxidant, 15 parts of curing agent, 2 parts of diluent and 2 parts of leveling agent, wherein samarium oxide, gadolinium oxide, cerium oxide and barium titanate powder are all in powder form.
[0028] The antioxidant is a phenol antioxidant, specifically 2,6-di-tert-butylphenol (BHT), the curing agent is an aromatic amine curing agent diethyltoluenediamine, the diluent is polyol glycidyl ether, the leveling agent is silicone oil, and the epoxy resin is bisphenol A epoxy resin.
[0029] A method for preparing a composite electromagnetic absorbing material comprises the following steps:
[0030] Step 1: Material preparation
[0031] According to the formula, weigh 60 parts of magnetite powder, 5 parts of nickel powder, 5 parts of copper powder, 2 parts of samarium oxide, 2 parts of gadolinium oxide, 2 parts of cerium oxide, 7 parts of carbon black powder, 8 parts of graphite powder, 20 parts of epoxy resin, 7 parts of barium titanate powder, 2 parts of antioxidant, 15 parts of curing agent, 2 parts of diluent and 2 parts of leveling agent;
[0032] Step 2: Mixing of absorbing magnetic materials
[0033] The magnetite powder, nickel powder and copper powder are ground by an ultrafine powder grinder respectively, and then added into a dry powder mixer, and then graphite powder, carbon black powder and barium titanate powder are added and stirred to obtain a wave absorbing magnetic material, wherein the particle size of the magnetite powder, nickel powder and copper powder is controlled within 5 μm by the ultrafine powder grinder;
[0034] Step 3: Mixing of rare earth materials
[0035] The samarium oxide, gadolinium oxide and cerium oxide are dried in a vacuum drying oven, and then mixed in a dry powder mixer to obtain a mixed rare earth oxide material, wherein the vacuum drying oven drying parameters are: temperature 120° C., drying time 10 min;
[0036] Step 4: Preparation of composite electromagnetic absorbing materials
[0037] The epoxy resin and the curing agent are stirred and mixed in a heating environment, wherein the heating environment is 80° C., and then a diluent is added and stirred continuously to obtain a mixed matrix, and then the absorbing magnetic material in step 2 and the mixed rare earth oxide material in step 3 are added and mixed again. During the mixing process, an antioxidant and a leveling agent are added and mixed for ultrasonic dispersion to obtain a composite electromagnetic absorbing material.
[0038] In this embodiment, the remaining parameters are the same as those in the third embodiment.
[0039] Embodiment 2
[0040] according to Figure 1As shown, this embodiment proposes a composite electromagnetic absorbing material, including the following raw materials in parts by weight: including the following raw materials in parts by weight: 50 parts of magnetite powder, 8 parts of nickel powder, 8 parts of copper powder, 4 parts of samarium oxide, 4 parts of gadolinium oxide, 4 parts of cerium oxide, 5 parts of carbon black powder, 15 parts of graphite powder, 30 parts of epoxy resin, 5 parts of barium titanate powder, 1 part of antioxidant, 20 parts of curing agent, 1 part of diluent and 1 part of leveling agent, samarium oxide, gadolinium oxide, cerium oxide and barium titanate powder are all in powder form, the antioxidant is a phenolic antioxidant, the curing agent is an aromatic amine curing agent diethyltoluene diamine, the diluent is polyol glycidyl ether, the leveling agent is silicone oil, and the epoxy resin is bisphenol A epoxy resin.
[0041] A method for preparing a composite electromagnetic absorbing material comprises the following steps:
[0042] Step 1: Material preparation
[0043] According to the formula, weigh 50 parts of magnetite powder, 8 parts of nickel powder, 8 parts of copper powder, 4 parts of samarium oxide, 4 parts of gadolinium oxide, 4 parts of cerium oxide, 5 parts of carbon black powder, 15 parts of graphite powder, 30 parts of epoxy resin, 5 parts of barium titanate powder, 1 part of antioxidant, 20 parts of curing agent, 1 part of diluent and 1 part of leveling agent;
[0044] Step 2: Mixing of absorbing magnetic materials
[0045] The magnetite powder, nickel powder and copper powder are ground by an ultrafine powder grinder respectively, and then added into a dry powder mixer, and then graphite powder, carbon black powder and barium titanate powder are added and stirred to obtain a wave absorbing magnetic material, wherein the particle size of the magnetite powder, nickel powder and copper powder is controlled to 2 μm by the ultrafine powder grinder;
[0046] Step 3: Mixing of rare earth materials
[0047] The samarium oxide, gadolinium oxide and cerium oxide are dried in a vacuum drying oven, and then mixed in a dry powder mixer to obtain a mixed rare earth oxide material, wherein the vacuum drying oven drying parameters are: temperature 90°C, drying time 20min;
[0048] Step 4: Preparation of composite electromagnetic absorbing materials
[0049] The epoxy resin and the curing agent are stirred and mixed in a heating environment, wherein the heating environment is 60°C, and then a diluent is added and stirred continuously to obtain a mixed matrix, and then the absorbing magnetic material in step 2 and the mixed rare earth oxide material in step 3 are added and mixed again. During the mixing process, an antioxidant and a leveling agent are added and mixed for ultrasonic dispersion to obtain a composite electromagnetic absorbing material.
[0050] In this embodiment, the remaining parameters are the same as those in the third embodiment.
[0051] Embodiment 3
[0052] according to Figure 1 As shown, this embodiment proposes a composite electromagnetic absorbing material, including the following raw materials in parts by weight: 55 parts of magnetite powder, 7 parts of nickel powder, 7 parts of copper powder, 3 parts of samarium oxide, 3 parts of gadolinium oxide, 3 parts of cerium oxide, 6 parts of carbon black powder, 10 parts of graphite powder, 26 parts of epoxy resin, 6 parts of barium titanate powder, 1 part of antioxidant, 18 parts of curing agent, 1 part of diluent and 1 part of leveling agent, samarium oxide, gadolinium oxide, cerium oxide and barium titanate powder are all in powder form, the antioxidant is a phenolic antioxidant, the curing agent is an aromatic amine curing agent diethyltoluene diamine, the diluent is polyol glycidyl ether, the leveling agent is silicone oil, and the epoxy resin is bisphenol A epoxy resin.
[0053] A method for preparing a composite electromagnetic absorbing material comprises the following steps:
[0054] Step 1: Material preparation
[0055] According to the formula, weigh 55 parts of magnetite powder, 7 parts of nickel powder, 7 parts of copper powder, 3 parts of samarium oxide, 3 parts of gadolinium oxide, 3 parts of cerium oxide, 6 parts of carbon black powder, 10 parts of graphite powder, 26 parts of epoxy resin, 6 parts of barium titanate powder, 1 part of antioxidant, 18 parts of curing agent, 1 part of diluent and 1 part of leveling agent;
[0056] Step 2: Mixing of absorbing magnetic materials
[0057] The magnetite powder, nickel powder and copper powder are respectively ground by an ultrafine powder grinder. The particle size of the magnetite powder, nickel powder and copper powder is controlled at 3 μm by the ultrafine powder grinder. By reducing the particle size of the powder to the micron level, the specific surface area of the powder can be increased, thereby improving its dispersibility in the composite material and the contact area with the matrix, which is helpful to improve the electromagnetic properties of the material. At the same time, the refined powder particles are more easily dispersed evenly in the matrix material, reducing agglomeration. Then, after grinding, the powder is added to a dry powder mixer, and graphite powder, carbon black powder and barium titanate powder are added and stirred for 8 minutes to obtain a wave-absorbing magnetic material.
[0058] Step 3: Mixing of rare earth materials
[0059] The samarium oxide, gadolinium oxide and cerium oxide are dried in a vacuum drying oven, wherein the vacuum drying oven drying parameters are: temperature 100°C, drying time 12 minutes, the purpose of drying is mainly to remove the moisture absorbed by the rare earth materials during storage and transportation, and after drying, they are mixed in a dry powder mixer, and after mixing for 5 minutes, a mixed rare earth oxide material is obtained;
[0060] Step 4: Preparation of composite electromagnetic absorbing materials
[0061] The epoxy resin and the curing agent are stirred and mixed in a heating environment, wherein the heating environment is 70° C. Specifically, the epoxy resin is added into a mixer and heated to 70° C., the curing agent is added, and stirring is started to mix evenly, and then the diluent is added and stirred continuously to facilitate the dispersion and mixing of the filler, and then a mixed matrix is obtained, and then the absorbing magnetic material in step 2 and the mixed rare earth oxide material in step 3 are added and mixed again for 15 minutes. Antioxidants and leveling agents are added during the mixing process. This mixing is preliminary mixing, that is, it has a pre-dispersion effect. After the mixing, the mixed materials are placed in an ultrasonic disperser for ultrasonic dispersion. Ultrasonic dispersion technology can be used to help the filler to be evenly dispersed in the epoxy resin, and the preliminary mixing method can reduce the ultrasonic dispersion time, and then play an effect of improving the preparation efficiency. After ultrasonic dispersion, a composite electromagnetic absorbing material is obtained, and further molding, curing and corresponding post-treatment are performed as needed. In this embodiment, the power of the ultrasonic disperser is 1500W, the ultrasonic frequency is 20 kHz, and the ultrasonic dispersion time is 30 minutes.
[0062] In combination with Example 1, Example 2 and Example 3, in the present invention, a composite electromagnetic absorbing material is used, with magnetite powder as the main body, and a small amount of nickel powder and copper powder are added for compounding. The magnetic loss characteristics of magnetite powder, the ferromagnetic behavior of nickel powder and the conductivity of copper powder are combined, which is conducive to achieving good electromagnetic wave absorption performance. Graphite powder and carbon black powder are introduced as conductive fillers and added to the absorbing material to improve the conductivity of the material, thereby improving impedance matching and enhancing the absorbing effect. Barium titanate powder is a material with a high dielectric constant. It can improve the dielectric loss of the composite material and contribute to the absorption of electromagnetic waves. At the same time, it also has good thermal stability. Further, the mixed rare earth oxide is introduced, that is, the rare earth doping method is used to improve the absorbing characteristics of the composite electromagnetic material, that is, the absorption amount is increased, the bandwidth is expanded, and the matching thickness is thinned. In the present invention, epoxy resin is used as an adhesive. As a thermosetting resin, it has a strong bonding ability and can firmly bond various fillers in the absorbing material together to form a stable composite material.
[0063] The composite electromagnetic absorbing materials provided in Example 1, Example 2 and Example 3 were measured using a vector network analyzer, and compared with a control group (the control group was a common ferrite absorbing material purchased on the market), the test results were as follows:
[0064]
[0065] As shown in the above table, the composite electromagnetic material provided by the present invention has good wave absorbing properties.
[0066] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the framework and scope of application of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A composite electromagnetic absorbing material, characterized in that: The invention comprises the following raw materials in parts by weight: 50-60 parts of magnetite powder, 5-8 parts of nickel powder, 5-8 parts of copper powder, 2-4 parts of samarium oxide, 2-4 parts of gadolinium oxide, 2-4 parts of cerium oxide, 5-7 parts of carbon black powder, 8-15 parts of graphite powder, 20-30 parts of epoxy resin, 5-7 parts of barium titanate powder, 1-2 parts of antioxidant, 15-20 parts of curing agent, 1-2 parts of diluent and 1-2 parts of leveling agent, wherein the samarium oxide, gadolinium oxide, cerium oxide and barium titanate powder are all in powder form, the antioxidant is a phenolic antioxidant, the curing agent is an aromatic amine curing agent diethyltoluenediamine, the diluent is polyol glycidyl ether, the leveling agent is silicone oil, and the epoxy resin is bisphenol A epoxy resin.
2. The composite electromagnetic absorbing material according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: 60 parts of magnetite powder, 5 parts of nickel powder, 5 parts of copper powder, 2 parts of samarium oxide, 2 parts of gadolinium oxide, 2 parts of cerium oxide, 7 parts of carbon black powder, 8 parts of graphite powder, 20 parts of epoxy resin, 7 parts of barium titanate powder, 2 parts of antioxidant, 15 parts of curing agent, 2 parts of diluent and 2 parts of leveling agent.
3. The composite electromagnetic absorbing material according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: 50 parts of magnetite powder, 8 parts of nickel powder, 8 parts of copper powder, 4 parts of samarium oxide, 4 parts of gadolinium oxide, 4 parts of cerium oxide, 5 parts of carbon black powder, 15 parts of graphite powder, 30 parts of epoxy resin, 5 parts of barium titanate powder, 1 part of antioxidant, 20 parts of curing agent, 1 part of diluent and 1 part of leveling agent.
4. A method for preparing a composite electromagnetic absorbing material according to claim 1, characterized in that: The following steps are involved: Step 1: Material preparation According to the formula, weigh 50-60 parts of magnetite powder, 5-8 parts of nickel powder, 5-8 parts of copper powder, 2-4 parts of samarium oxide, 2-4 parts of gadolinium oxide, 2-4 parts of cerium oxide, 5-7 parts of carbon black powder, 8-15 parts of graphite powder, 20-30 parts of epoxy resin, 5-7 parts of barium titanate powder, 1-2 parts of antioxidant, 15-20 parts of curing agent, 1-2 parts of diluent and 1-2 parts of leveling agent; Step 2: Mixing of absorbing magnetic materials Grinding magnetite powder, nickel powder and copper powder, adding graphite powder, carbon black powder and barium titanate powder and stirring to obtain a wave-absorbing magnetic material; Step 3: Mixing of rare earth materials drying samarium oxide, gadolinium oxide and cerium oxide and mixing them to obtain a mixed rare earth oxide material; Step 4: Preparation of composite electromagnetic absorbing materials The epoxy resin and the curing agent are stirred and mixed under a heating environment, and then a diluent is added and stirred continuously to obtain a mixed matrix, and then the absorbing magnetic material in step 2 and the mixed rare earth oxide material in step 3 are added and mixed again. During the mixing process, an antioxidant and a leveling agent are added and mixed for ultrasonic dispersion to obtain a composite electromagnetic absorbing material.
5. The method for preparing a composite electromagnetic absorbing material according to claim 4, characterized in that: In the step 2, the particle sizes of magnetite powder, nickel powder and copper powder are controlled to be 2-5 μm by using an ultra-fine powder grinder.
6. The method for preparing a composite electromagnetic absorbing material according to claim 4, characterized in that: The drying is vacuum drying, and the parameters are: temperature 90-120° C., and drying time 10-20 min.
7. The method for preparing a composite electromagnetic absorbing material according to claim 4, characterized in that: In the step 4, the heating environment is 60-80°C.