A high-strength antibacterial mortar material and its preparation method and application

By using Cu2O/ZrO2/sermica composite material and nano-copper modified chitin fibers in mortar materials, combined with cement and epoxy resin, the problems of poor antibacterial effect and reduced strength of existing antibacterial mortar materials have been solved, and high Improved strength and long-term antibacterial properties.

CN118637875BActive Publication Date: 2024-12-06BEIJING ECO HOME (LETING) TECH DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411110521.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-12-06
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The existing antibacterial mortar materials have low antibacterial effects, short duration, and the addition of antibacterial agents lead to a decrease in the strength of the material, making it difficult to meet the long-term antibacterial needs.

Method used

Cement and epoxy resins are used as cementitious materials, combined with Cu2O/ZrO2/sermica composite material and nano-copper modified chitin fibers, enhance antibacterial performance through the interaction between cuprous oxide and the surface of bacterial cell and copper ion association. , and improve material strength through tailings powder and quartz sand.

Benefits of technology

It achieves good compressive strength and flexural strength of high-strength antibacterial mortar materials, while significantly improving antibacterial properties, extending antibacterial effects, and providing longer-lasting antibacterial properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention relates to the technical field of building materials, and specifically discloses a high-strength antibacterial mortar material and its preparation method and application. The high-strength antibacterial mortar material includes the following raw material components by mass: 75-95 parts of cement, 40-80 parts of tailings powder, 100-130 parts of quartz sand, 1-2 parts of water reducer, 3-5 parts of dispersant, 0.5-1 parts of stabilizer, 30-50 parts of Cu2O / ZrO2 / sericite composite material, 30-50 parts of nano-copper modified chitin fiber, 30-50 parts of epoxy resin and 70-100 parts of water. The high-strength antibacterial mortar material provided by the present invention has good compressive strength and flexural strength and excellent antibacterial performance, which can effectively solve the problems of poor antibacterial effect, short duration and decreased strength of mortar materials in the prior art.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and specifically discloses a high-strength antibacterial mortar material and a preparation method and application thereof. Background Art

[0002] Bacteria are everywhere. They can be in the air or attached to daily necessities we touch, posing a huge threat and harm to people's physical and mental health. These harmful bacteria often exist in bathtubs, toilets, sinks, bowls, plates, dishes, and various building materials, such as interior and exterior wall tiles and floor tiles. They are spread by a large number of people and cause infection with various pathogens, posing a threat to human health. Under the premise of continuous improvement of science and technology and people's quality of life, it is urgent to develop building materials with antibacterial properties.

[0003] Mortar materials are high-strength building materials that are mixed and hardened with cement, sand and fine aggregate as the main raw materials. They are mainly used for masonry, plastering and decorative construction projects. However, due to the certain porosity of mortar materials, bacteria are more likely to grow, which seriously affects environmental hygiene and even shortens the service life of mortar materials. In order to avoid this problem, engineers have developed antibacterial mortar materials, using antibacterial agents to kill or inhibit the growth of bacteria, or coating antibacterial coatings on the surface of mortar. However, the antibacterial rate of existing antibacterial mortar materials is relatively low, only about 60%, and the antibacterial effect lasts for a short time, which is difficult to meet the purpose of long-term antibacterial. What's more, due to the addition of antibacterial agents, the strength of mortar materials has decreased to varying degrees. Based on this, the development of a high-strength mortar material with excellent antibacterial effect is a major breakthrough in the field of antibacterial building materials. Summary of the invention

[0004] In view of the problems of poor antibacterial effect, short duration and decreased strength of antibacterial mortar materials in the prior art, the present invention provides a high-strength antibacterial mortar material and its preparation method and application. The high-strength antibacterial mortar material is prepared with cement and epoxy resin as gelling materials; tailings powder, quartz sand, Cu2O / ZrO2 / sericite composite material and nano-copper modified chitin fiber as aggregates; water reducer, dispersant and stabilizer as additives. The present invention utilizes the synergistic effect of each raw material component to make the obtained high-strength antibacterial mortar material have good compressive strength and flexural strength as well as excellent antibacterial properties.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The first aspect of the present invention provides a high-strength antibacterial mortar material, comprising the following raw material components in parts by weight: 75-95 parts of cement, 40-80 parts of tailings powder, 100-130 parts of quartz sand, 1-2 parts of water reducer, 3-5 parts of dispersant, 0.5-1 part of stabilizer, 30-50 parts of Cu2O / ZrO2 / sericite composite material, 30-50 parts of nano-copper modified chitin fiber, 30-50 parts of epoxy resin and 70-100 parts of water.

[0007] Cuprous oxide has high antiviral and antibacterial properties, and also has the ability to adsorb and denature proteins. When bacteria come into contact with cuprous oxide, Cu (I) complexes with the protein surface in the bacteria to inactivate the relevant active enzymes, thereby causing bacterial death and achieving the purpose of antibacterial. However, cuprous oxide is prone to agglomeration due to the interaction of Cu-Cu metal bonds, and has poor stability, and its antibacterial effect is greatly reduced after agglomeration. Based on this, the present invention uniformly loads cuprous oxide on sericite with a layered structure, effectively reducing the agglomeration rate of cuprous oxide. The present invention also introduces zirconium oxide on the basis of cuprous oxide, and uses zirconium oxide to assist in enhancing the interaction between cuprous oxide and the surface of bacterial cells, increasing the permeability of bacterial cell membranes, so that the interior of bacterial cells directly contacts cuprous oxide, thereby reducing the vitality of bacteria and achieving the purpose of strong antibacterial.

[0008] The present invention also designs a nano-copper modified chitin fiber. The chitin fiber itself has a certain antibacterial ability, but in fact its antibacterial efficiency in a neutral environment is not high. If it is directly applied to a mortar material, it cannot well improve the antibacterial properties of the mortar material. Therefore, the present invention performs a modification process on it, using nano-copper to load on chitin fiber, copper ions and hydroxyl and amino groups on the surface of chitin fiber form an association, thereby firmly fixing the nano-copper on the fiber surface. Both nano-copper and chitin fiber have a certain antibacterial ability, and the combination of the two greatly enhances this performance, effectively improving the antibacterial properties of the mortar material.

[0009] In order to avoid the problem of strength reduction while the antibacterial properties of the mortar material are enhanced, the present invention also uses tailings powder and quartz sand, which are fine aggregates with high strength and low porosity, combined with cement and epoxy resin as gelling materials and related auxiliary materials, to effectively reduce the pore density of the mortar material, thereby improving its strength. By utilizing the interaction of the various raw material components of the present invention, the obtained high-strength antibacterial mortar material has good compressive strength and flexural strength as well as excellent antibacterial properties, providing a new design idea for antibacterial building materials.

[0010] Preferably, the preparation method of the Cu2O / ZrO2 / sericite composite material comprises the following steps:

[0011] S1, dispersing sericite in an alcohol solution, performing ultrasonic treatment, filtering, adding the solid filtrate into an acidic oxidizing solution, activating at 90° C.-120° C., washing, and drying to obtain activated sericite;

[0012] S2. Disperse cuprous oxide and zirconium oxide in an organic solvent, mix well, add the activated sericite, carry out hydrothermal reaction at 170° C.-190° C. in an inert atmosphere, filter, and dry to obtain a Cu2O / ZrO2 / sericite composite material.

[0013] Further preferably, in S1, the particle size of the sericite is 20 μm-50 μm.

[0014] Further preferably, in S1, the ultrasonic treatment time is 25 min-45 min.

[0015] Further preferably, in S1, the alcohol solution is a 75%-85% methanol solution.

[0016] Further preferably, in S1, the acidic oxidizing solution is concentrated sulfuric acid and hydrogen peroxide in a volume ratio of 1:2-1.5:3.

[0017] Further preferably, in S1, the mass volume ratio of the sericite to the alcohol solution is 1 g:2 mL-1 g:3 mL.

[0018] Further preferably, in S1, the mass volume ratio of the sericite to the acidic oxidizing solution is 1 g:1 mL-1 g:2 mL.

[0019] Further preferably, in S1, the activation time is 6h-10h.

[0020] Further preferably, in S2, the mass ratio of cuprous oxide to zirconium oxide is 1:0.8-1:1.

[0021] More preferably, in S2, the organic solvent is triethanolamine.

[0022] Further preferably, in S2, the mass volume ratio of the cuprous oxide to the organic solvent is 1 g:1 mL-1 g:2 mL.

[0023] Further preferably, in S2, the mass ratio of the cuprous oxide to the activated sericite is 0.5:1-0.5:3.

[0024] Further preferably, in S2, the hydrothermal reaction time is 3h-5h.

[0025] Preferably, the preparation method of the nano-copper modified chitin fiber comprises the following steps:

[0026] Step a, mixing the reducing agent solution and the protective agent evenly to obtain a reducing-protecting mixed system; in an inert atmosphere, slowly dropping the copper ammonia solution into the reducing-protecting mixed system, and performing a reduction reaction at 100° C.-120° C. to obtain nano copper powder;

[0027] Step b, immersing chitin fiber in an alcohol solution, adding the nano copper powder, and performing a hydrothermal reaction in an inert atmosphere at 120° C.-140° C. to obtain nano copper modified chitin fiber.

[0028] Further preferably, in step a, the reducing agent solution is any one of a glucose solution, an ascorbic acid solution or a borate solution.

[0029] Further preferably, in step a, the protective agent is any one or both of polyvinyl pyrrolidone and polyvinyl alcohol.

[0030] Further preferably, in step a, the slow dripping rate is 1.5 mL / min-2.0 mL / min.

[0031] Further preferably, the concentration of the copper ammonia solution is 0.05 mol / L-0.01 mol / L.

[0032] Further preferably, in step a, the volume ratio of the copper ammonia solution to the reduction-protection mixed system is 1:2-1:3.

[0033] Further preferably, the mass volume ratio of the protective agent and the reducing agent solution in the reduction-protection mixed system is 0.05g:1mL-0.1g:1mL, wherein the concentration of the reducing agent solution is 0.02mol / L-0.05mol / L.

[0034] Further preferably, in step a, the reduction reaction time is 4h-8h.

[0035] Further preferably, in step b, the alcohol solution is a 65%-75% ethanol solution.

[0036] Further preferably, in step b, the mass volume ratio of the chitosan fiber to the alcohol solution is 1 g:2 mL-1 g:3 mL.

[0037] Further preferably, in step b, the mass ratio of the chitin fiber to the nano copper powder is 1:0.5-1:0.8.

[0038] Further preferably, in step b, the hydrothermal reaction time is 2h-4h.

[0039] Preferably, the cement is Portland cement.

[0040] Preferably, the particle size of the tailings powder is 0.3 mm-0.5 mm.

[0041] Preferably, the particle size of the quartz sand is 0.1 mm-0.3 mm.

[0042] Preferably, the water reducer is any one of a sodium lignin sulfonate water reducer, a naphthalene-based high-efficiency water reducer, an aliphatic high-efficiency water reducer, an amino high-efficiency water reducer or a polycarboxylic acid high-efficiency water reducer.

[0043] Preferably, the dispersant is a fatty acid dispersant.

[0044] Preferably, the stabilizer is any one of EL0002, TAB-2 or T-386.

[0045] The second aspect of the present invention provides a method for preparing the high-strength antibacterial mortar material, comprising the following steps: weighing each raw material component according to the designed ratio, and mixing the weighed components evenly to obtain the high-strength antibacterial mortar material.

[0046] The third aspect of the present invention provides the use of the high-strength antibacterial mortar material or the high-strength antibacterial mortar material prepared by the preparation method of the high-strength antibacterial mortar material in the field of building materials.

[0047] In summary, the present invention uses cement and epoxy resin as cementitious materials; uses tailings powder, quartz sand, Cu2O / ZrO2 / sericite composite materials and nano-copper modified chitin fibers as aggregates; and uses water reducer, dispersant and stabilizer as additives to prepare a high-strength antibacterial mortar material. The high-strength antibacterial mortar material has good compressive strength and flexural strength and excellent antibacterial properties. The use of the mortar material can effectively solve the problems of poor antibacterial effect, short duration and reduced strength of the antibacterial mortar material in the prior art. DETAILED DESCRIPTION

[0048] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0049] Example 1

[0050] This embodiment provides a high-strength antibacterial mortar material and a preparation method thereof, which specifically includes the following contents:

[0051] The high-strength antibacterial mortar material includes the following raw material components in parts by weight: 85 parts of silicate cement, 60 parts of tailings powder, 120 parts of quartz sand, 2 parts of sodium lignin sulfonate water reducer, 3 parts of fatty acid dispersant, 0.8 parts of EL0002 stabilizer, 40 parts of Cu2O / ZrO2 / sericite composite material, 50 parts of nano-copper modified chitin fiber, 40 parts of epoxy resin and 90 parts of water.

[0052] The raw material components are weighed according to the designed proportions, and the weighed components are evenly mixed to obtain a high-strength antibacterial mortar material.

[0053] The preparation method of the Cu2O / ZrO2 / sericite composite material comprises the following steps:

[0054] S1. Disperse 100 g of sericite with a particle size of 30 μm in 80% methanol solution and perform ultrasonic treatment for 35 min. Filter and add the solid filtrate into 200 mL of a mixed solution of concentrated sulfuric acid and hydrogen peroxide in a volume ratio of 1:2.5, activate at 100° C. for 8 h, wash and dry at 80° C. for 4 h to obtain activated sericite.

[0055] S2. Under an inert atmosphere, disperse 35 g of cuprous oxide and 30 g of zirconium oxide in 50 mL of triethanolamine, mix well, add 75 g of activated sericite, carry out hydrothermal reaction at 180 °C for 4 h, filter, wash, and dry at 90 °C for 3 h to obtain a Cu2O / ZrO2 / sericite composite material.

[0056] The preparation method of the nano-copper modified chitin fiber comprises the following steps:

[0057] Step a, 500mL of 0.4mol / L glucose solution and 40g of polyvinyl pyrrolidone are mixed evenly to obtain a reduction-protection mixed system; under an inert atmosphere, 110mL of 0.08mol / L copper ammonia solution is slowly added dropwise to the reduction-protection mixed system at a drop rate of 1.8mL / min, and a reduction reaction is carried out at 110°C for 6h, filtered, and dried to obtain nano copper powder;

[0058] Step b: 80 g of chitosan fiber was immersed in 200 mL of 70% ethanol solution, 30 g of the nano copper powder was added under an inert atmosphere, and a hydrothermal reaction was carried out at 130° C. for 3 h to obtain nano copper modified chitosan fiber.

[0059] The particle size of the tailings powder is 0.4 mm; the particle size of the quartz sand is 0.2 mm.

[0060] Example 2

[0061] This embodiment provides a high-strength antibacterial mortar material and a preparation method thereof, which specifically includes the following contents:

[0062] The high-strength antibacterial mortar material includes the following raw material components in parts by weight: 90 parts of silicate cement, 75 parts of tailings powder, 110 parts of quartz sand, 1.5 parts of naphthalene-based high-efficiency water reducer, 3 parts of fatty acid dispersant, 1 part of TAB-2 stabilizer, 45 parts of Cu2O / ZrO2 / sericite composite material, 45 parts of nano-copper modified chitin fiber, 45 parts of epoxy resin and 85 parts of water.

[0063] The raw material components are weighed according to the designed proportions, and the weighed components are evenly mixed to obtain a high-strength antibacterial mortar material.

[0064] The preparation method of the Cu2O / ZrO2 / sericite composite material comprises the following steps:

[0065] S1. Disperse 100 g of sericite with a particle size of 30 μm in 80% methanol solution and perform ultrasonic treatment for 35 min. Filter and add the solid filtrate into 200 mL of a mixed solution of concentrated sulfuric acid and hydrogen peroxide in a volume ratio of 1:2.5, activate at 100° C. for 8 h, wash and dry at 80° C. for 4 h to obtain activated sericite.

[0066] S2. Under an inert atmosphere, disperse 35 g of cuprous oxide and 30 g of zirconium oxide in 50 mL of triethanolamine, mix well, add 75 g of activated sericite, carry out hydrothermal reaction at 180 °C for 4 h, filter, wash, and dry at 90 °C for 3 h to obtain a Cu2O / ZrO2 / sericite composite material.

[0067] The preparation method of the nano-copper modified chitin fiber comprises the following steps:

[0068] Step a, 500mL of 0.4mol / L glucose solution and 40g of polyvinyl pyrrolidone are mixed evenly to obtain a reduction-protection mixed system; under an inert atmosphere, 110mL of 0.08mol / L copper ammonia solution is slowly added dropwise to the reduction-protection mixed system at a drop rate of 1.5mL / min, and a reduction reaction is carried out at 110°C for 6h, filtered, and dried to obtain nano copper powder;

[0069] Step b: 80 g of chitosan fiber was immersed in 200 mL of 70% ethanol solution, 30 g of the nano copper powder was added under an inert atmosphere, and a hydrothermal reaction was carried out at 130° C. for 3 h to obtain nano copper modified chitosan fiber.

[0070] The particle size of the tailings powder is 0.3 mm; the particle size of the quartz sand is 0.3 mm.

[0071] Example 3

[0072] This embodiment provides a high-strength antibacterial mortar material and a preparation method thereof, which specifically includes the following contents:

[0073] The high-strength antibacterial mortar material includes the following raw material components in parts by weight: 75 parts of silicate cement, 45 parts of tailings powder, 130 parts of quartz sand, 1 part of amino high-efficiency water reducing agent, 5 parts of fatty acid dispersant, 0.5 parts of T-386 stabilizer, 35 parts of Cu2O / ZrO2 / sericite composite material, 35 parts of nano-copper modified chitin fiber, 50 parts of epoxy resin and 85 parts of water.

[0074] The raw material components are weighed according to the designed proportions, and the weighed components are evenly mixed to obtain a high-strength antibacterial mortar material.

[0075] The preparation method of the Cu2O / ZrO2 / sericite composite material comprises the following steps:

[0076] S1. Disperse 100 g of sericite with a particle size of 30 μm in 80% methanol solution and perform ultrasonic treatment for 35 min. Filter and add the solid filtrate into 200 mL of a mixed solution of concentrated sulfuric acid and hydrogen peroxide in a volume ratio of 1:2.5, activate at 100° C. for 8 h, wash and dry at 80° C. for 4 h to obtain activated sericite.

[0077] S2. Under an inert atmosphere, disperse 35 g of cuprous oxide and 30 g of zirconium oxide in 50 mL of triethanolamine, mix well, add 75 g of activated sericite, carry out hydrothermal reaction at 180 °C for 4 h, filter, wash, and dry at 90 °C for 3 h to obtain a Cu2O / ZrO2 / sericite composite material.

[0078] The preparation method of the nano-copper modified chitin fiber comprises the following steps:

[0079] Step a, 500mL of 0.4mol / L glucose solution and 40g of polyvinyl pyrrolidone are mixed evenly to obtain a reduction-protection mixed system; under an inert atmosphere, 110mL of 0.08mol / L copper ammonia solution is slowly added dropwise to the reduction-protection mixed system at a drop rate of 2.0mL / min, and a reduction reaction is carried out at 110°C for 6h, filtered, and dried to obtain nano copper powder;

[0080] Step b: 80 g of chitosan fiber was immersed in 200 mL of 70% ethanol solution, 30 g of the nano copper powder was added under an inert atmosphere, and a hydrothermal reaction was carried out at 130° C. for 3 h to obtain nano copper modified chitosan fiber.

[0081] The particle size of the tailings powder is 0.5 mm; the particle size of the quartz sand is 0.1 mm.

[0082] Comparative Example 1

[0083] This comparative example provides a high-strength antibacterial mortar material and a preparation method thereof, which is different from Example 1 in that the Cu2O / ZrO2 / sericite composite material is replaced by an equal amount of Cu2O / sericite composite material, and other components and processes remain unchanged, specifically including the following contents:

[0084] The high-strength antibacterial mortar material includes the following raw material components in parts by weight: 85 parts of silicate cement, 60 parts of tailings powder, 120 parts of quartz sand, 2 parts of sodium lignin sulfonate water reducer, 3 parts of fatty acid dispersant, 0.8 parts of EL0002 stabilizer, 40 parts of Cu2O / sericite composite material, 50 parts of nano-copper modified chitin fiber, 40 parts of epoxy resin and 90 parts of water.

[0085] The raw material components are weighed according to the designed proportions, and the weighed components are evenly mixed to obtain a high-strength antibacterial mortar material.

[0086] The preparation method of the Cu2O / sericite composite material comprises the following steps:

[0087] S1. Disperse 100 g of sericite with a particle size of 30 μm in 80% methanol solution and perform ultrasonic treatment for 35 min. Filter and add the solid filtrate into 200 mL of a mixed solution of concentrated sulfuric acid and hydrogen peroxide in a volume ratio of 1:2.5, activate at 100° C. for 8 h, wash and dry at 80° C. for 4 h to obtain activated sericite.

[0088] S2. Under an inert atmosphere, 35 g of cuprous oxide was dispersed in 50 mL of triethanolamine, mixed evenly, 75 g of activated sericite was added, and a hydrothermal reaction was carried out at 180 °C for 4 h. The mixture was filtered, washed, and dried at 90 °C for 3 h to obtain a Cu2O / sericite composite material.

[0089] The preparation method of the nano-copper modified chitin fiber comprises the following steps:

[0090] Step a, 500mL of 0.4mol / L glucose solution and 40g of polyvinyl pyrrolidone are mixed evenly to obtain a reduction-protection mixed system; under an inert atmosphere, 110mL of 0.08mol / L copper ammonia solution is slowly added dropwise to the reduction-protection mixed system at a drop rate of 1.8mL / min, and a reduction reaction is carried out at 110°C for 6h, filtered, and dried to obtain nano copper powder;

[0091] Step b: 80 g of chitosan fiber was immersed in 200 mL of 70% ethanol solution, 30 g of the nano copper powder was added under an inert atmosphere, and a hydrothermal reaction was carried out at 130° C. for 3 h to obtain nano copper modified chitosan fiber.

[0092] The particle size of the tailings powder is 0.4 mm; the particle size of the quartz sand is 0.2 mm.

[0093] Comparative Example 2

[0094] This comparative example provides a high-strength antibacterial mortar material and a preparation method thereof, which is different from Example 1 in that the Cu2O / ZrO2 / sericite composite material is replaced by an equal amount of ZrO2 / sericite composite material, and other components and processes remain unchanged, specifically including the following contents:

[0095] The high-strength antibacterial mortar material includes the following raw material components in parts by weight: 85 parts of silicate cement, 60 parts of tailings powder, 120 parts of quartz sand, 2 parts of sodium lignin sulfonate water reducer, 3 parts of fatty acid dispersant, 0.8 parts of EL0002 stabilizer, 40 parts of ZrO2 / sericite composite material, 50 parts of nano-copper modified chitin fiber, 40 parts of epoxy resin and 90 parts of water.

[0096] The preparation method of the ZrO2 / sericite composite material comprises the following steps:

[0097] S1. Disperse 100 g of sericite with a particle size of 30 μm in 80% methanol solution and perform ultrasonic treatment for 35 min. Filter and add the solid filtrate into 200 mL of a mixed solution of concentrated sulfuric acid and hydrogen peroxide in a volume ratio of 1:2.5, activate at 100° C. for 8 h, wash and dry at 80° C. for 4 h to obtain activated sericite.

[0098] S2. Under an inert atmosphere, disperse 30 g of zirconium oxide in 50 mL of triethanolamine, mix well, add 75 g of activated sericite, perform hydrothermal reaction at 180 °C for 4 h, filter, wash, and dry at 90 °C for 3 h to obtain a ZrO2 / sericite composite material.

[0099] The preparation method of the nano-copper modified chitin fiber comprises the following steps:

[0100] Step a, 500mL of 0.4mol / L glucose solution and 40g of polyvinyl pyrrolidone are mixed evenly to obtain a reduction-protection mixed system; under an inert atmosphere, 110mL of 0.08mol / L copper ammonia solution is slowly added dropwise to the reduction-protection mixed system at a drop rate of 1.8mL / min, and a reduction reaction is carried out at 110°C for 6h, filtered, and dried to obtain nano copper powder;

[0101] Step b: 80 g of chitosan fiber was immersed in 200 mL of 70% ethanol solution, 30 g of the nano copper powder was added under an inert atmosphere, and a hydrothermal reaction was carried out at 130° C. for 3 h to obtain nano copper modified chitosan fiber.

[0102] The particle size of the tailings powder is 0.4 mm; the particle size of the quartz sand is 0.2 mm.

[0103] Comparative Example 3

[0104] This comparative example provides a high-strength antibacterial mortar material and a preparation method thereof, which is different from Example 1 in that the nano-copper modified chitin fiber is replaced with an equal amount of chitin fiber, and other components and processes remain unchanged, specifically including the following contents:

[0105] The high-strength antibacterial mortar material includes the following raw material components in parts by weight: 85 parts of silicate cement, 60 parts of tailings powder, 120 parts of quartz sand, 2 parts of sodium lignin sulfonate water reducer, 3 parts of fatty acid dispersant, 0.8 parts of EL0002 stabilizer, 40 parts of Cu2O / ZrO2 / sericite composite material, 50 parts of chitin fiber, 40 parts of epoxy resin and 90 parts of water.

[0106] The raw material components are weighed according to the designed proportions, and the weighed components are evenly mixed to obtain a high-strength antibacterial mortar material.

[0107] The preparation method of the Cu2O / ZrO2 / sericite composite material comprises the following steps:

[0108] S1. Disperse 100 g of sericite with a particle size of 30 μm in 80% methanol solution and perform ultrasonic treatment for 35 min. Filter and add the solid filtrate into 200 mL of a mixed solution of concentrated sulfuric acid and hydrogen peroxide in a volume ratio of 1:2.5, activate at 100° C. for 8 h, wash and dry at 80° C. for 4 h to obtain activated sericite.

[0109] S2. Under an inert atmosphere, disperse 35 g of cuprous oxide and 30 g of zirconium oxide in 50 mL of triethanolamine, mix well, add 75 g of activated sericite, carry out hydrothermal reaction at 180 °C for 4 h, filter, wash, and dry at 90 °C for 3 h to obtain a Cu2O / ZrO2 / sericite composite material.

[0110] The particle size of the tailings powder is 0.4 mm; the particle size of the quartz sand is 0.2 mm.

[0111] In order to further reflect the technical effect of the present invention, the present invention conducted the following tests on the mortar materials obtained in Examples 1-3 and Comparative Examples 1-3: the compressive strength and flexural strength were tested with reference to the standard of GB / T17671-2021, and the results are shown in Table 1;

[0112] The present invention also conducts antibacterial tests on the mortar materials obtained in Examples 1-3 and Comparative Examples 1-3. The specific operations are as follows: the mortar materials are made into 6cm×6cm×3cm mortar blocks for antibacterial experiments, which are placed in sealable containers respectively, and the test objects containing Staphylococcus aureus, Escherichia coli, Streptococcus, Pseudomonas aeruginosa, and Candida albicans are evenly applied to the surface of the mortar blocks. After being sealed and allowed to stand for 30 minutes at 25°C, antibacterial testing is performed. The results are shown in Table 2; after being sealed and allowed to stand for 90 days at 25°C, antibacterial testing is performed, and the results are shown in Table 3.

[0113] Table 1 Test results of compression and flexural properties of various mortar materials

[0114]

[0115] Table 2 Antibacterial test results of mortar materials after standing for 30 minutes

[0116]

[0117] Table 3 Antibacterial test results of mortar materials after standing for 90 days

[0118]

[0119] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A high-strength antibacterial mortar material, characterized in that: The invention comprises the following raw material components in parts by weight: 75-95 parts of cement, 40-80 parts of tailings powder, 100-130 parts of quartz sand, 1-2 parts of water reducer, 3-5 parts of dispersant, 0.5-1 part of stabilizer, 30-50 parts of Cu2O / ZrO2 / sericite composite material, 30-50 parts of nano-copper modified chitin fiber, 30-50 parts of epoxy resin and 70-100 parts of water; The preparation method of the Cu2O / ZrO2 / sericite composite material comprises the following steps: S1, dispersing sericite in an alcohol solution, performing ultrasonic treatment, filtering, adding the solid filtrate into an acidic oxidizing solution, activating at 90° C.-120° C., washing, and drying to obtain activated sericite; S2. Disperse cuprous oxide and zirconium oxide in an organic solvent, mix well, add the activated sericite, carry out hydrothermal reaction at 170° C.-190° C. in an inert atmosphere, filter, and dry to obtain a Cu2O / ZrO2 / sericite composite material. The preparation method of the nano-copper modified chitin fiber comprises the following steps: Step a, mixing the reducing agent solution and the protective agent evenly to obtain a reducing-protecting mixed system; in an inert atmosphere, slowly dropping the copper ammonia solution into the reducing-protecting mixed system, and performing a reduction reaction at 100° C.-120° C. to obtain nano copper powder; Step b, immersing chitin fiber in an alcohol solution, adding the nano copper powder, and performing a hydrothermal reaction in an inert atmosphere at 120° C.-140° C. to obtain nano copper modified chitin fiber.

2. The high-strength antibacterial mortar material according to claim 1, characterized in that: In S1, the particle size of the sericite is 20 μm-50 μm; and / or In S1, the ultrasonic treatment time is 25min-45min; and / or In S1, the alcohol solution is a 75%-85% methanol solution; and / or In S1, the acidic oxidizing solution is concentrated sulfuric acid and hydrogen peroxide in a volume ratio of 1:2-1.5:

3.

3. The high-strength antibacterial mortar material according to claim 1, characterized in that: In S1, the mass volume ratio of the sericite to the alcohol solution is 1 g:2 mL-1 g:3 mL; and / or In S1, the mass volume ratio of the sericite to the acidic oxidizing solution is 1 g:1 mL-1 g:2 mL; and / or In S1, the activation time is 6h-10h.

4. The high-strength antibacterial mortar material according to claim 1, characterized in that: In S2, the mass ratio of cuprous oxide to zirconium oxide is 1:0.8-1:1; and / or In S2, the organic solvent is triethanolamine; and / or In S2, the mass volume ratio of the cuprous oxide to the organic solvent is 1 g:1 mL-1 g:2 mL; and / or In S2, the mass ratio of the cuprous oxide to the activated sericite is 0.5:1-0.5:3; and / or In S2, the hydrothermal reaction time is 3h-5h.

5. The high-strength antibacterial mortar material according to claim 1, characterized in that: In step a, the reducing agent solution is any one of a glucose solution, an ascorbic acid solution or a borate solution; and / or In step a, the protective agent is any one or both of polyvinyl pyrrolidone and polyvinyl alcohol; and / or In step a, the slow dripping rate is 1.5 mL / min-2.0 mL / min; and / or In step a, the concentration of the copper ammonia solution is 0.05 mol / L-0.01 mol / L; and / or In step a, the volume ratio of the copper ammonia solution to the reduction-protection mixed system is 1:2-1:3; and / or In step a, the mass volume ratio of the protective agent and the reducing agent solution in the reduction-protection mixed system is 0.05g:1mL-0.1g:1mL, wherein the concentration of the reducing agent solution is 0.02mol / L-0.05mol / L; and / or In step a, the reduction reaction time is 4h-8h.

6. The high-strength antibacterial mortar material according to claim 1, characterized in that: In step b, the alcohol solution is a 65%-75% ethanol solution; and / or In step b, the mass volume ratio of the chitin fiber to the alcohol solution is 1g:2mL-1g:3mL; and / or In step b, the mass ratio of the chitin fiber to the nano copper powder is 1:0.5-1:0.8; and / or In step b, the hydrothermal reaction time is 2h-4h.

7. The method for preparing the high-strength antibacterial mortar material according to any one of claims 1 to 6, characterized in that: The method comprises the following steps: weighing various raw material components according to the designed proportion, and uniformly mixing the weighed components to obtain a high-strength antibacterial mortar material.

8. Use of the high-strength antibacterial mortar material according to any one of claims 1 to 6 or the high-strength antibacterial mortar material prepared by the preparation method of the high-strength antibacterial mortar material according to claim 7 in the field of building materials.