A high oxygen permeability silicone hydrogel material and its preparation method and application
Through the chemical modification and polymerization of new silicon-containing raw materials, combined with photoinitiation technology, a high-oxygen permeability silicon hydrogel material was prepared, which solved the problems of insufficient oxygen permeability and low antibacterial performance of traditional contact lens materials, and achieved significant improvements The effect of oxygen permeability and antibacterial properties is suitable for the manufacturing of long-term wear contact lenses.
Patent Information
- Application Number
- CN202411111164.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-14
AI Technical Summary
Traditional contact lens materials such as HEMA hydrogels are insufficient in long-term wear, resulting in corneal hypoxia. The existing silicone hydrogel materials still have room for improvement in antibacterial performance and comfort, especially when worn for a long time. It is difficult to ensure the stability and safety of the material.
Compound 1 is obtained by chemical modification of new silicon-containing raw materials, and the highly oxygen permeable silicone hydrogel material is prepared by polymerization with monomers such as 2-hydroxyethyl methacrylate, 1-vinyl-2-pyrrolidone, glycerol and other monomers. , combined with the preparation process of photoinitiation technology, a material with excellent oxygen permeability, strong antibacterial properties and good biocompatibility is formed.
It significantly improves the oxygen permeability and antibacterial properties of contact lenses, enhances wear comfort, ensures the stability and safety of the material, and is suitable for the manufacturing of long-term wear contact lenses.
Smart Images

Figure CN118638279B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of silicone hydrogel materials, and in particular relates to a high oxygen permeable silicone hydrogel material and a preparation method and application thereof. Background Art
[0002] With the continuous advancement of medical technology and the increasing attention paid to eye health, contact lenses, as an important means of vision correction, have a growing market demand. However, traditional contact lens materials such as HEMA hydrogel often cause corneal hypoxia due to insufficient oxygen permeability during long-term wear, which in turn causes discomfort symptoms such as red eyes, dryness, blurred vision, and may even cause more serious eye diseases such as keratitis and conjunctivitis. Therefore, the development of new contact lens materials with high oxygen permeability, good biocompatibility, antibacterial properties and wearing comfort has become a research hotspot in the current fields of optometry and materials science.
[0003] Traditional hydrogel materials, such as HEMA hydrogel, transfer oxygen through water molecules, and their oxygen permeability is limited by the water content. However, although high water content can increase oxygen permeability, it will also reduce the formability and stability of the lens, and may even absorb moisture from the eyes, causing discomfort when wearing. Silicone hydrogel materials stand out because of their unique molecular structure and excellent oxygen permeability. By introducing silicone monomers, silicone hydrogel significantly improves the oxygen permeability of the material while maintaining the high water content of the hydrogel material, thereby effectively alleviating the problem of corneal hypoxia. However, the existing silicone hydrogel materials on the market still need to be improved in terms of antibacterial properties and comfort. Especially in the context of long-term wear, how to ensure the stability and safety of the material's oxygen permeability and antibacterial properties has become a technical problem that needs to be solved urgently.
[0004] In view of the deficiencies in the prior art, the present invention aims to provide a novel high oxygen permeability silicone hydrogel material and a preparation method and application thereof, which provides a new solution for preparing corneal contact lenses with high oxygen permeability, hydrophilicity, antibacterial properties and biocompatibility. Summary of the invention
[0005] The first object of the present invention is to provide a highly oxygen permeable silicone hydrogel material, which is prepared by chemically modifying a novel silicon-containing raw material to obtain compound 1, and then polymerizing it with monomers such as 2-hydroxyethyl methacrylate, 1-vinyl-2-pyrrolidone, and glycerol. The silicone hydrogel material of the present invention has excellent oxygen permeability and exhibits strong antibacterial properties, and is particularly suitable for making contact lenses, which can significantly improve wearing comfort.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] A method for preparing a high oxygen permeable silicone hydrogel material comprises the following steps:
[0008] S1. Prepare compound 1, whose structural formula is:
[0009]
[0010] S2. Preparation of high oxygen permeability silicone hydrogel materials
[0011] Compound 1, 2-hydroxyethyl methacrylate, 1-vinyl-2-pyrrolidone, glycerol and a photoinitiator are mixed to obtain a mixed solution, the mixed solution is added into a mold, and after standing for forming, photoinitiation, demolding and post-treatment are performed to obtain the product.
[0012] Furthermore, the preparation of compound 1 comprises the following steps:
[0013]
[0014] (1) adding γ-aminopropylmethyldiethoxysilane and N-[2-(3,4-dihydroxyphenyl)ethyl]-2-acrylamide to anhydrous ethanol and stirring for reaction. After the reaction is completed, the reaction solution is purified to obtain intermediate 1;
[0015] (2) adding intermediate 1 and 3-formylphenylboronic acid into a solvent and stirring for reaction. After the reaction is completed, the reaction solution is purified to obtain intermediate 2;
[0016] (3) adding intermediate 2 and but-3-enoyl chloride to acetone for reaction. After the reaction is completed, the reaction solution is post-treated to obtain intermediate 3;
[0017] (4) Chitosan quaternary ammonium salt and intermediate 3 are added to a solvent for reaction. After the reaction is completed, the reaction solution is post-treated to obtain compound 1.
[0018] Furthermore, in step (1), the molar ratio of γ-aminopropylmethyldiethoxysilane to N-[2-(3,4-dihydroxyphenyl)ethyl]-2-acrylamide is 1:1-1.5, and the stirring reaction time is 115-125 hours.
[0019] Furthermore, in step (2), the molar ratio of the intermediate 1 to 3-formylphenylboronic acid is 1:1.2-2, and the stirring reaction time is 23-25 hours.
[0020] Furthermore, in step (3), the molar ratio of the intermediate 2 to but-3-enoyl chloride is 1:2-3, the reaction temperature is 50-60° C., and the reaction time is 5-7 h.
[0021] Furthermore, in step (4), the mass ratio of the chitosan quaternary ammonium salt to the intermediate 3 is 1:0.2-0.5, and the reaction time is 11-13 hours.
[0022] Furthermore, the mass ratio of the compound 1, 2-hydroxyethyl methacrylate, 1-vinyl-2-pyrrolidone, glycerol and photoinitiator is 1: (1-2): (0.25-0.4): (0.05-0.2): (0.02-0.03).
[0023] Furthermore, the photoinitiation process is: irradiation under ultraviolet light of 5 mW / cm and 365 nm for 200-230 min, and the photoinitiator is phenyl (2,4,6-trimethylbenzoyl) lithium phosphate.
[0024] The second object of the present invention is to provide a method for preparing a highly oxygen-permeable silicone hydrogel material, which has a simple and controllable process and is easy for industrial production.
[0025] In order to achieve the above object, the technical solution adopted by the present invention is:
[0026] A high oxygen permeability silicone hydrogel material is prepared according to the above preparation method.
[0027] The third purpose of the present invention is to provide an application of a high oxygen permeable silicone hydrogel material in the preparation of corneal contact lenses. The product has stable performance and has broad application prospects in the field of biomedical materials, and is particularly suitable for the manufacture of long-term wear contact lenses.
[0028] In order to achieve the above object, the technical solution adopted by the present invention is:
[0029] Application of the above-mentioned high oxygen permeability silicone hydrogel material in the preparation of corneal contact lenses.
[0030] Compared with the prior art, the beneficial effects of the present invention are mainly:
[0031] 1. The present invention provides a highly oxygen permeable silicone hydrogel material, which is prepared by chemically modifying a novel silicon-containing raw material to obtain compound 1, and then reacting the compound with 2-hydroxyethyl methacrylate, 1-vinyl-2-pyrrolidone, glycerol and other monomers through polymerization. Experimental results show that the silicone hydrogel material prepared by the present invention has the following properties: (1) Excellent oxygen permeability, which has certain potential in the manufacture of contact lenses. (2) Strong antibacterial properties: Through the introduction of specific functional groups during the synthesis process, the silicone hydrogel has strong antibacterial properties. (3) Excellent biocompatibility: The MTT experimental results show that the silicone hydrogel material prepared by the present invention has good biocompatibility and can avoid irritation to eye tissues when used as contact lenses.
[0032] 2. The present invention provides a method for preparing a highly oxygen-permeable silicone hydrogel material, which has a simple and controllable process and is easy for industrial production.
[0033] 3. The present invention provides the use of the high oxygen permeability silicone hydrogel material prepared by the above method in the preparation of corneal contact lenses. The product has stable performance and is particularly suitable for the manufacture of long-term wear contact lenses. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 are SEM images of the materials obtained in the present invention, wherein Figures a to d are SEM images of the high oxygen permeability silicone hydrogel materials obtained in Examples 1-3 and the silicone hydrogel material obtained in Comparative Example 1, respectively;
[0035] Figure 2 This is a diagram showing the sterilization effect of the material obtained by the present invention;
[0036] Figure 3 This is a graph showing the biocompatibility results of the material obtained in the present invention. DETAILED DESCRIPTION
[0037] The technical scheme of the present invention is further described below in conjunction with specific embodiments. However, it should be understood by those skilled in the art that the following examples are only used to illustrate the present invention and should not be regarded as limiting the present invention. The specific conditions not specified in the examples are carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, unless otherwise specified, are conventional products obtained through commercial channels.
[0038] Example 1
[0039] S1. Preparation of compound 1:
[0040]
[0041] (1) γ-aminopropylmethyldiethoxysilane (10 mmol) and N-[2-(3,4-dihydroxyphenyl)ethyl]-2-acrylamide (10 mmol) were added to 200 mL of anhydrous ethanol and stirred for 120 h. After the reaction was completed, the reaction solution was concentrated, dried, and purified by column chromatography to obtain intermediate 1;
[0042] (2) Add intermediate 1 (10 mmol) and 3-formylphenylboronic acid (12 mmol) to 200 mL of ethanol / water mixed solvent (volume ratio of 9:1), stir and react for 24 h. After the reaction is completed, extract the reaction solution, collect the organic phase and purify it by concentration, drying and column chromatography to obtain intermediate 2;
[0043] (3) Dissolve the intermediate 2 (10 mmol) in 100 mL of anhydrous acetone. After complete dissolution, add but-3-enoyl chloride (20 mmol) and reflux at 55 °C for 6 h. After the reaction is completed, add excess water to terminate the reaction and precipitate the crude product. Collect the crude product and dissolve it in acetone, then add water again to precipitate it. Repeat this process three times to obtain the purified intermediate 3.
[0044] (4) Dissolve 1 g of chitosan quaternary ammonium salt in 50 mL of ethanol / water (volume ratio of 1:1) mixed solvent, adjust the pH to 8.2, and then add 0.35 g of intermediate 3. After reacting for 12 h, add anhydrous ethanol to the system to precipitate the product, thereby obtaining compound 1;
[0045] S2. Preparation of high oxygen permeability silicone hydrogel material:
[0046] 4g of compound 1 was mixed with 4g of 2-hydroxyethyl methacrylate (HEMA), 1g of 1-vinyl-2-pyrrolidone (NVP), 0.5g of glycerol, and 0.08g of phenyl (2,4,6-trimethylbenzoyl) lithium phosphate (LAP) to obtain a mixed solution, which was added to a contact lens mold, allowed to stand for 1h to form, and then irradiated with 5 mW / cm ultraviolet light (365 nm) for 220min. After demolding, the obtained gel was soaked in a 50% ethanol solution at 50°C for 20h to remove unreacted monomers and photoinitiators. The gel was then soaked in distilled water at 50°C for 4h to remove ethanol, and the gel was stored in PBS buffer (pH7.4) at room temperature for later use.
[0047] Example 2
[0048] S1. Preparation of compound 1:
[0049]
[0050] (1) γ-aminopropylmethyldiethoxysilane (10 mmol) and N-[2-(3,4-dihydroxyphenyl)ethyl]-2-acrylamide (12.5 mmol) were added to 200 mL of anhydrous ethanol and stirred for 115 h. After the reaction was completed, the reaction solution was concentrated, dried, and purified by column chromatography to obtain intermediate 1;
[0051] (2) Add intermediate 1 (10 mmol) and 3-formylphenylboronic acid (15 mmol) to 200 mL of ethanol / water mixed solvent (volume ratio of 9:1), stir and react for 23 h. After the reaction is completed, extract the reaction solution, collect the organic phase and purify it by concentration, drying and column chromatography to obtain intermediate 2;
[0052] (3) Dissolve the intermediate 2 (10 mmol) in 100 mL of anhydrous acetone. After complete dissolution, add but-3-enoyl chloride (25 mmol) and reflux at 50 °C for 7 h. After the reaction is completed, add excess water to terminate the reaction and precipitate the crude product. Collect the crude product and dissolve it in acetone, then add water again to precipitate it. Repeat this process three times to obtain the purified intermediate 3.
[0053] (4) 1 g of chitosan quaternary ammonium salt was dissolved in 50 mL of ethanol / water (volume ratio 1:1) mixed solvent, the pH was adjusted to 8.2, and 0.2 g of intermediate 3 was added thereto. After reacting for 11 h, anhydrous ethanol was added to the system to precipitate the product, thereby obtaining compound 1;
[0054] S2. Preparation of high oxygen permeability silicone hydrogel material:
[0055] 4g of compound 1 was mixed with 6g of HEMA, 1.2g of NVP, 0.2g of glycerol, and 0.1g of LAP to obtain a mixed solution, which was added to a contact lens mold, allowed to stand for 1h to form, and then irradiated with 5 mW / cm ultraviolet light (365 nm) for 200min. After demolding, the resulting gel was soaked in a 50% ethanol solution at 50°C for 20h to remove unreacted monomers and photoinitiators. The gel was then soaked in 50°C distilled water for 4h to remove ethanol, and the gel was stored in PBS buffer (pH 7.4) at room temperature for later use.
[0056] Example 3
[0057] S1. Preparation of compound 1:
[0058]
[0059] (1) γ-aminopropylmethyldiethoxysilane (10 mmol) and N-[2-(3,4-dihydroxyphenyl)ethyl]-2-acrylamide (15 mmol) were added to 200 mL of anhydrous ethanol and stirred for reaction for 125 h. After the reaction was completed, the reaction solution was concentrated, dried, and purified by column chromatography to obtain intermediate 1;
[0060] (2) Add intermediate 1 (10 mmol) and 3-formylphenylboronic acid (20 mmol) to 200 mL of ethanol / water mixed solvent (volume ratio of 9:1), stir and react for 25 h. After the reaction is completed, extract the reaction solution, collect the organic phase and purify it by concentration, drying and column chromatography to obtain intermediate 2;
[0061] (3) Dissolve the intermediate 2 (10 mmol) in 100 mL of anhydrous acetone. After complete dissolution, add but-3-enoyl chloride (30 mmol) and reflux at 60 °C for 5 h. After the reaction is completed, add excess water to terminate the reaction and precipitate the crude product. Collect the crude product and dissolve it in acetone, then add water again to precipitate it. Repeat this process three times to obtain the purified intermediate 3.
[0062] (4) Dissolve 1 g of chitosan quaternary ammonium salt in 50 mL of ethanol / water (volume ratio of 1:1) mixed solvent, adjust the pH to 8.2, and then add 0.5 g of intermediate 3. After reacting for 13 h, add anhydrous ethanol to the system to precipitate the product to obtain compound 1;
[0063] S2. Preparation of high oxygen permeability silicone hydrogel material:
[0064] 4g of compound 1 was mixed with 8g of HEMA, 1.6g of NVP, 0.8g of glycerol, and 0.12g of LAP to obtain a mixed solution, which was added to a contact lens mold, allowed to stand for 1h to form, and then irradiated with 5 mW / cm ultraviolet light (365 nm) for 230min. After demolding, the resulting gel was soaked in a 50% ethanol solution at 50°C for 20h to remove unreacted monomers and photoinitiators. The gel was then soaked in 50°C distilled water for 4h to remove ethanol, and the gel was stored in PBS buffer (pH 7.4) at room temperature for later use.
[0065] Comparative Example 1
[0066] Comparative Example 1 provides a silicone hydrogel, the steps are as follows: 4g of γ-aminopropylmethyldiethoxysilane is mixed with 4g of 2-hydroxyethyl methacrylate (HEMA), 1g of 1-vinyl-2-pyrrolidone (NVP), 0.5g of glycerol, 0.1g of ethylene glycol dimethacrylate, and 0.08g of phenyl (2,4,6-trimethylbenzoyl) lithium phosphate (LAP) to obtain a mixed solution, the mixed solution is added to a contact lens mold, and the mold is formed by standing for 1 hour, and then irradiated with ultraviolet light (365 nm) of 5 mW / cm for 220 minutes. After demolding, the obtained gel is soaked in a 50% ethanol solution at 50°C for 20 hours to remove unreacted monomers and photoinitiators. Then the gel is soaked in 50°C distilled water for 4 hours to remove ethanol, and the gel is stored in PBS buffer (pH7.4) at room temperature for standby use.
[0067] The properties of the high oxygen permeability silicone hydrogel material prepared by the present invention are further described below.
[0068] Test Example 1
[0069] Surface morphology test: The microstructure of the materials obtained in Examples 1-3 and Comparative Example 1 was tested using a scanning electron microscope. The results are as follows: Figure 1 As shown, Figures a to d are SEM images of the high oxygen permeability silicone hydrogel materials obtained in Examples 1-3 and the silicone hydrogel material obtained in Comparative Example 1, respectively.
[0070] Depend on Figure 1 It can be seen that the high oxygen permeability silicone hydrogel materials obtained in Examples 1-3 of the present invention and the silicone hydrogel material obtained in Comparative Example 1 both have smooth surfaces, indicating that the introduction of compound 1 into the high oxygen permeability silicone hydrogel material obtained in Example 1 does not change its microstructure, so its surface is smooth and has no cracks.
[0071] Test Example 2
[0072] Equilibrium water content test: The prepared hydrogel sample was placed in deionized water and soaked for 2 consecutive days. Fresh deionized water was replaced every day. After it reached swelling equilibrium, it was taken out and the residual water on the surface was gently absorbed with filter paper and weighed. Then the hydrogel sample was placed in a vacuum drying oven at 50°C until it reached constant weight. The sample was taken out and weighed immediately. Five samples were taken from each group for testing, and the average value was taken as the final experimental result. The equilibrium water content (EWC) formula is as follows: EWC (%) = (W 1 -W 2 ) / W 1 , where W 1 represents the mass of the hydrogel at swelling equilibrium, W 2 is the mass of the hydrogel dried to constant weight; the experimental results are shown in Table 1.
[0073] Test Example 3
[0074] Wettability test: A contact angle meter (DSA 100, Germany) was used to test the surface wettability of the products obtained in Examples 1-3 and Comparative Example 1. The specific steps are as follows:
[0075] The hydrogels obtained in Examples 1-3 and Comparative Example 1 were first immersed in deionized water for 48 h, and then the residual water on the surface was wiped off and fixed on a glass slide using double-sided tape. Deionized water (5 µL) was dripped on the surface of each sample, and then the contact angle value of each sample was measured and recorded one by one using a contact angle meter. Each group of samples was measured 5 times, and the average value was taken as the final result. The experimental results are shown in Table 1.
[0076] Test Example 4
[0077] Oxygen permeability test: In order to evaluate the oxygen permeability of the hydrogels obtained in Examples 1-3 and Comparative Example 1, an oxygen permeability tester (PERME OX2 / 230) was used to conduct the experiment. Specifically, the above hydrogels were immersed in physiological saline for 48 hours, and the oxygen permeability of each group of hydrogels was measured at 37°C and 90% relative humidity under simulated human physiological conditions according to the national standard GB / T 11417.3-2012. Each group of samples was tested three times, and the average value was calculated as the basis for the final evaluation of oxygen permeability. The experimental results are shown in Table 1.
[0078] Table 1
[0079]
[0080] As can be seen from Table 1, the contact angles of the hydrogels obtained in Examples 1-3 all vary around 50°, which may be due to the introduction of the novel silicon-containing material (prepared by chemically modifying γ-aminopropylmethyldiethoxysilane) used in the present invention, namely, compound 1, which gives the hydrogel good hydrophilicity. The contact angle of comparative example 1 is significantly higher than that of example 1, further illustrating that the introduction of compound 1 can significantly improve the hydrophilicity of the highly oxygen permeable silicone hydrogel material.
[0081] In addition, the introduction of the new silicon-containing material Compound 1 makes the equilibrium water content of the hydrogels of Examples 1-3 significantly higher than that of Comparative Example 1. Specifically, the equilibrium water content of the hydrogels of Examples 1-3 is maintained at about 50%, while that of Comparative Example 1 is only about 35%. The above results show that the high oxygen permeability silicone hydrogel material prepared by the present invention has a certain wearing comfort and can be worn for a long time.
[0082] The oxygen permeability coefficient (DK) represents the oxygen permeability of the hydrogel material, as shown in Table 1: the oxygen permeability coefficients of Examples 1-3 are significantly higher than that of Comparative Example 1. This is because the present invention obtains Compound 1 by chemically modifying γ-aminopropylmethyldiethoxysilane. When Compound 1 is introduced into the hydrogel matrix, it can significantly increase the equilibrium water content of the hydrogel, thereby enhancing the oxygen permeability of the hydrogel.
[0083] Test Example 5
[0084] Antibacterial performance: The hydrogels prepared in Examples 1-3 and Comparative Example 1 were placed in physiological saline and soaked for 48 hours (thickness 1 mm), and then the hydrogel samples were made into 1 cm × 1 cm squares, the moisture on the surface of the hydrogels was wiped off, and the samples were placed on a clean bench and sterilized by ultraviolet light for 2 hours.
[0085] The concentration was 1×10 8CFU / mL of Staphylococcus aureus suspension was used as the experimental strain, and 1 mL of the above experimental strain was added to a 24-well plate containing the highly oxygen-permeable silicone hydrogel material obtained in Example 1, as Example 1 group. Similarly, the silicone hydrogels obtained in Examples 2-3 and Comparative Example 1 were co-cultured with the above Staphylococcus aureus suspension, as Example 2 group, Example 3 group, and Comparative Example 1 group; at the same time, a blank control group was set up: 1 mL of Staphylococcus aureus suspension was added to the wells without silicone hydrogel. The 24-well plate inoculated with the strain was placed in a 37°C constant temperature shaker, the speed was adjusted to 100 rpm, and incubated for 2 hours. 1 mL of physiological saline was added thereto, and ultrasound (power 80w, frequency 40KHz) was used for 15 seconds, and then the bacterial suspension was diluted to 1×10 4 CFU / mL, 50 μL of bacterial suspension was taken from each group and spread on the surface of sterile agar medium, which was placed in a 37°C constant temperature incubator for 1 day, and the number of colonies was recorded. Sterilization rate (%) = (number of colonies in the blank control group - number of colonies in the sample group) / number of colonies in the blank control group × 100%, the sterilization rate value is the average of 3 parallel experiments, the results are shown in Figure 2 .
[0086] Long-term wearing of contact lenses can easily lead to the growth of microorganisms in the eyes, which in turn aggravates existing eye diseases. However, the use of contact lenses with antibacterial properties can effectively reduce the occurrence of such problems. Figure 2 As shown: the high oxygen permeable silicone hydrogel materials prepared in Examples 1-3 have a good inhibition rate against Staphylococcus aureus, which can reach more than 90%. The antibacterial performance of Comparative Example 1 is the worst, indicating that the high oxygen permeable silicone hydrogel materials obtained in Examples 1-3 have good antibacterial performance, which may be attributed to the introduction of compound 1 giving the silicone hydrogel material good antibacterial properties.
[0087] Test Example 6
[0088] Cytotoxicity test: The hydrogels obtained in Examples 1-3 and Comparative Example 1 were sterilized under ultraviolet light for 12 h, and human corneal epithelial cells (HCECs) were cultured at a rate of 5×10 4 The cells were inoculated into a 96-well plate at a density of 100 / mL and incubated in a cell culture incubator for 12 hours. The sterilized hydrogels of Examples 1-3 and Comparative Example 1 were added to each well and cultured together for 48 hours as a sample group. After the culture was completed, the culture medium was aspirated, and 100 µL of MTT reagent was added to the culture medium of the above-mentioned cells and cultured in a 37°C incubator for 4 hours. Then, dimethyl sulfoxide (DMSO) was added to the culture medium to dissolve the purple product, and the culture was incubated at 37°C and 5% for 48 hours. Finally, the absorbance value at 490 nm was detected by an ELISA instrument. The experimental results are shown in FIG. Figure 3 shown.
[0089] Cell survival rate (%) = (absorbance value of sample group / absorbance value of blank group) × 100%
[0090] Depend on Figure 3 The results show that after incubation for 48 hours, the cell survival rates of the hydrogels in Examples 1-3 of the present invention and Comparative Example 1 were all above 96%, indicating that the highly oxygen-permeable silicone hydrogel material prepared by the present invention has no cytotoxicity and is suitable for preparing contact lenses suitable for long-term wear.
[0091] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them. The basic principles and main features of the present invention have been described above with specific implementation schemes. On the basis of the present invention, some modifications or replacements may be made thereto, but these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of protection claimed by the present invention.
Claims
1. A method for preparing a highly oxygen permeable silicone hydrogel material, characterized in that: The steps include: S1. Prepare compound 1, whose structural formula is: The vertical wavy line in the formula represents the molecular skeleton of chitosan; S2. Preparation of highly oxygen permeable silicone hydrogel materials Compound 1, 2-hydroxyethyl methacrylate, 1-vinyl-2-pyrrolidone, glycerol and a photoinitiator are mixed to obtain a mixed solution, the mixed solution is added into a mold, and after standing for forming, photoinitiation, demolding and post-treatment are performed to obtain the product.
2. The method for preparing the high oxygen permeability silicone hydrogel material according to claim 1, characterized in that: The preparation of compound 1 comprises the following steps: (1) adding γ-aminopropylmethyldiethoxysilane and N-[2-(3,4-dihydroxyphenyl)ethyl]-2-acrylamide to ethanol and stirring for reaction. After the reaction is completed, the reaction solution is purified to obtain intermediate 1; (2) adding intermediate 1 and 3-formylphenylboronic acid into a solvent and stirring for reaction. After the reaction is completed, the reaction solution is purified to obtain intermediate 2; (3) adding intermediate 2 and but-3-enoyl chloride to acetone for reaction. After the reaction is completed, the reaction solution is post-treated to obtain intermediate 3; (4) Chitosan quaternary ammonium salt and intermediate 3 are added to a solvent for reaction. After the reaction is completed, the reaction solution is post-treated to obtain compound 1.
3. The method for preparing the high oxygen permeability silicone hydrogel material according to claim 2, characterized in that: In step (1), the molar ratio of γ-aminopropylmethyldiethoxysilane to N-[2-(3,4-dihydroxyphenyl)ethyl]-2-acrylamide is 1:1-1.5, and the stirring reaction time is 115-125 hours.
4. The method for preparing the high oxygen permeability silicone hydrogel material according to claim 2, characterized in that: In step (2), the molar ratio of the intermediate 1 to 3-formylphenylboronic acid is 1:1.2-2, and the stirring reaction time is 23-25 hours.
5. The method for preparing the high oxygen permeability silicone hydrogel material according to claim 2, characterized in that: In step (3), the molar ratio of the intermediate 2 to but-3-enoyl chloride is 1:2-3, the reaction temperature is 50-60°C, and the reaction time is 5-7h.
6. The method for preparing the high oxygen permeability silicone hydrogel material according to claim 2, characterized in that: In step (4), the mass ratio of the chitosan quaternary ammonium salt to the intermediate 3 is 1:0.2-0.5, and the reaction time is 11-13 hours.
7. The method for preparing the high oxygen permeability silicone hydrogel material according to claim 1, characterized in that: The mass ratio of the compound 1, 2-hydroxyethyl methacrylate, 1-vinyl-2-pyrrolidone, glycerol and photoinitiator is 1: (1-2): (0.25-0.4): (0.05-0.2): (0.02-0.03).
8. The method for preparing the high oxygen permeability silicone hydrogel material according to claim 1, characterized in that: The photoinitiator process is: irradiating under 5 mW / cm, 365 nm ultraviolet light for 200-230 min, and the photoinitiator is phenyl (2,4,6-trimethylbenzoyl) lithium phosphate.
9. A highly oxygen permeable silicone hydrogel material, characterized in that: Prepared according to the preparation method according to any one of claims 1 to 8.
10. Use of the high oxygen permeable silicone hydrogel material according to claim 9 in the preparation of corneal contact lenses.
Citation Information
Cited By
Oxygen-permeable silica hydrogel material for contact lenses and preparation method of oxygen-permeable silica hydrogel material
CN120118253A