A polymer moisture-proof and fire-proof sealing composite material and preparation method thereof

By adding toughening repair components and weather-resistant components to the fire-resistant sealing material, the chemical bonding and hydrogen bonding of functionalized nanosilica and cellulose nanocrystals are solved, and the problem of poor brittleness and compatibility of epoxy resin is solved. The material's weather resistance, fire resistance and moisture resistance are improved, and higher mechanical properties and stability are achieved.

CN118638392BActive Publication Date: 2024-11-08YANTAI JINRUN NUCLEAR POWER MATERIAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411095019.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-08
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

Due to the brittleness and prone to cracking in fire-resistant sealing materials, existing epoxy resins have insufficient structural stability and service reliability, and are poorly compatible with liquid butadiene rubber, which affects its mechanical and bending resistance.

Method used

Using a polymer moisture-proof and fire-proof sealing combination material, the structural reinforcement material of cellulose nanocrystals is combined with cellulose nanocrystals by adding toughening repair components and weather-resistant components to the material. Weather resistance, improves the mechanical and fire resistance of the material, and enhances its weather resistance and moisture resistance through chemical bonding and hydrogen bonding.

Benefits of technology

The weather resistance, fire resistance and moisture resistance of the sealing composite materials are significantly improved, their mechanical properties are enhanced, compatibility and cross-linking with epoxy resin are improved, and the stability and reliability of the material are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present application relates to the technical field of plugging materials, and specifically discloses a polymer moisture-proof and fire-proof plugging composite material and a preparation method thereof, comprising the following raw materials in parts by weight: 55-70 parts of a matrix epoxy resin, 8-10 parts of a weather-resistant component, 12-16 parts of a toughening and repairing component, 5-10 parts of a diluent, 2-5 parts of a leveling agent, 1.2-1.5 parts of an accelerator, 16-18 parts of a curing agent, and 0.6-0.8 parts of a photoinitiator; the present application adds a weather-resistant component and a toughening and repairing component, the weather-resistant component is a cellulose nanocrystal grafted with 2-mercaptonicotinic acid, the outer layer of the toughening and repairing component is a polyhydroxy monomer structure obtained by chemical crosslinking of dihydroxy phosphate and terminal carboxyl polybutadiene, and the inner core contains functionalized nano-silica; through the combined action of the above structures, the weather resistance, fire resistance, moisture resistance and mechanical properties of the plugging composite material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of plugging materials, and more specifically, to a polymer moisture-proof and fire-proof plugging composite material and a preparation method thereof. Background Art

[0002] Fireproof sealing of large electrical appliances and cables is one of the key measures to ensure the safe operation of electrical equipment. With the acceleration of global urbanization and the improvement of public safety awareness, people have higher requirements for fireproof seals of large electrical appliances and cables.

[0003] Among the various existing polymer matrices, epoxy resin is widely used in fireproof sealing of large electrical appliances and cables due to its excellent mechanical, electrical and heat resistance properties. However, epoxy resin has problems such as high thermal expansion coefficient, inherent brittleness and easy cracking when heated, which are particularly prominent in the application of fireproof sealing, affecting the structural stability and service reliability of fireproof sealing materials.

[0004] In the prior art, epoxy resin and liquid butadiene rubber with low viscosity, high fluidity and high electrical insulation are blended to improve the above problems. However, the compatibility between liquid butadiene rubber and epoxy resin is poor. At the same time, the mechanical strength, bending resistance and aging resistance of liquid butadiene rubber itself are poor, which affects its performance in certain high-demand application scenarios. Summary of the invention

[0005] In order to solve the problems of poor compatibility between liquid butadiene rubber and epoxy resin, poor mechanical strength, bending resistance and aging performance of liquid butadiene rubber itself, the present application provides a sealing composite material with high weather resistance, good fire resistance, good moisture resistance and excellent mechanical properties.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A polymer moisture-proof and fire-proof sealing composite material, comprising the following raw materials in parts by weight: 55-70 parts of base epoxy resin, 8-10 parts of weather-resistant components, 12-16 parts of toughening and repairing components, 5-10 parts of diluents, 2-5 parts of leveling agents, 1.2-1.5 parts of accelerators, 16-18 parts of curing agents and 0.6-0.8 parts of photoinitiators;

[0008] The preparation method of the polymer moisture-proof and fire-proof sealing composite material comprises the following steps:

[0009] Step S1, mixing the base epoxy resin, toughening and repairing component, diluent and leveling agent uniformly, and preparing component A after vacuum degassing;

[0010] Step S2, uniformly mixing the weather-resistant component, the accelerator, the curing agent and the photoinitiator to prepare component B;

[0011] Step S3, encapsulating the combination A and the component B separately to obtain a polymer moisture-proof and fire-proof sealing composite material.

[0012] Preferably, in step S1, the base epoxy resin is bisphenol A epoxy resin or bisphenol F epoxy resin.

[0013] Preferably, the diluent is ethylene glycol diglycidyl ether.

[0014] Preferably, the leveling agent is polyether silicone oil JF-956.

[0015] Preferably, the accelerator is accelerator K-54.

[0016] Preferably, the curing agent is polyetheramine D230.

[0017] Preferably, in step S2, the photoinitiator is dimethyl benzoate.

[0018] Preferably, the weather-resistant component is prepared by the following steps:

[0019] Step A1, mixing microcrystalline cellulose and sulfuric acid solution evenly, maintaining the rotation speed unchanged, heating to 55-65° C., stirring for reaction for 2-4 hours, then adding deionized water, standing for 4-6 hours, precipitating, removing the supernatant, centrifuging the remaining suspension, dialyzing, and freeze-drying to obtain cellulose nanocrystals, using microcrystalline cellulose as a raw material, preparing cellulose nanocrystals by sulfuric acid hydrolysis, wherein the mass ratio of microcrystalline cellulose, sulfuric acid solution and deionized water is 1:13-15:40-60;

[0020] Step A2, adding cellulose nanocrystals, 2-mercaptonicotinic acid and trifluoromethanesulfonic acid to anhydrous DMF, stirring evenly, heating to 90-110° C. and stirring for reaction for 18-20 hours under nitrogen protection, standing for 4-6 hours after the reaction, filtering, washing the filter cake, and drying to obtain a weather-resistant component, wherein the mass ratio of cellulose nanocrystals, 2-mercaptonicotinic acid, trifluoromethanesulfonic acid and anhydrous DMF is 1:14-16:0.1-0.2:95-105. In the above reaction process, the hydroxyl groups on the surface of the cellulose nanocrystals are esterified with the 2-mercaptonicotinic acid to graft the weather-resistant components containing ester groups and mercapto groups onto the surface of the cellulose nanocrystals.

[0021] Preferably, in step A1, the mass fraction of the sulfuric acid solution is 62-66%.

[0022] Preferably, in step A1, the pore size of the dialysis bag used in the dialysis process is 120-160 kDa, and the dialysis time is 3.5-4.5 h.

[0023] Preferably, the toughening and repairing component is prepared by the following steps:

[0024] Step B1, carbon tetrachloride and tetrahydrofuran are mixed evenly, dibutyl phosphite is added, and triethylamine and ethanolamine are added under an ice-water bath, the temperature is raised to 45-55° C., the reaction is stirred for 8-10 hours, suction filtered, and the filtrate is rotary evaporated to obtain dihydroxy phosphate, wherein the mass ratio of carbon tetrachloride, tetrahydrofuran, dibutyl phosphite, triethylamine and ethanolamine is 70-80:35-45:4-6:1.5-2.1:2.2-3.2. In the above reaction process, dibutyl phosphite and ethanolamine are used as raw materials to obtain a compound containing two hydroxyl groups, one secondary amine group and a phosphate ester group, namely dihydroxy phosphate, through a Michael addition reaction;

[0025] The structural formula of the dihydroxy phosphate is shown below:

[0026]

[0027] Step B2, under nitrogen protection, add terminal carboxyl polybutadiene and dihydroxy phosphate to tetrahydrofuran, stir evenly, then add dicyclohexylcarbodiimide and 4-dimethylaminopyridine, heat to reflux, stir and react for 4-6 hours, after the reaction is completed, cool to room temperature, filter with suction, wash the filter cake, freeze-dry to obtain a polyhydroxy monomer, wherein the mass ratio of terminal carboxyl polybutadiene, dihydroxy phosphate, tetrahydrofuran, dicyclohexylcarbodiimide and 4-dimethylaminopyridine is 1:2.4-3.2:30-50:2.3-2.5:1.4-1.8, in the above reaction process, with tetrahydrofuran as solvent, dicyclohexylcarbodiimide as dehydrating agent, 4-dimethylaminopyridine as acylating agent, the terminal carboxyl polybutadiene and dihydroxy phosphate undergo amidation reaction to obtain a polyhydroxy monomer;

[0028] Step B3, adding polyhydroxy monomer and functionalized nano-silica to anhydrous toluene, stirring for reaction for 1-2 hours, filtering, and drying to obtain a toughening and repairing component, wherein the mass ratio of polyhydroxy monomer, functionalized nano-silica and anhydrous toluene is 12-16:1-3:60-70. During the above reaction process, the active hydroxyl groups on the surface of the polyhydroxy monomer can produce hydrogen bonds with the amino groups on the surface of the functionalized nano-silica, and then be coated on the surface of the functionalized nano-silica to obtain a toughening and repairing component.

[0029] Preferably, the number average molecular weight of the carboxyl-terminated polybutadiene is 2200-2600, and the carboxyl value is 0.04-0.06.

[0030] Preferably, the functionalized nano-silicon dioxide is prepared by the following steps:

[0031] Step C1, placing the nano-silica in a vacuum drying oven at 80°C and drying for 24 hours, then placing it in a mixture of anhydrous ethanol and deionized water a, ultrasonically crushing it for 0.5-1h, stirring it evenly, and when the temperature is constant, adding a mixture of KH-560 and anhydrous ethanol b dropwise, after the dropping is completed, heating it to 60-70°C, stirring and reacting for 4-6 hours, after the reaction is completed, cooling it to room temperature, centrifuging, washing, and drying it to obtain epoxy nano-silica, wherein the nano-silica, the mixture a and the mixture b are The mass ratio of the mixed solution b is 5:40-50:12-14, the mass ratio of anhydrous ethanol to deionized water in the mixed solution a is 20-24:10, and the mass ratio of KH-560 to anhydrous ethanol in the mixed solution b is 0.3-0.5:10. In the above reaction process, nano-silicon dioxide is modified by KH-560, which not only improves the dispersibility and compatibility of nano-silicon dioxide, but also obtains epoxy nano-silicon dioxide with epoxy groups on the surface, which paves the way for subsequent reactions;

[0032] Step C2, adding epoxy nano-silica to anhydrous DMF, stirring evenly, adding tetrabutylammonium bromide, DL-lipoic acid and anhydrous DMF mixed solution c dropwise while stirring, heating to 105-115°C after the addition is completed, stirring and reacting for 2-3 hours, centrifuging after the reaction is completed, washing the precipitate, and drying to obtain modified nano-silica, wherein the mass ratio of epoxy nano-silica, anhydrous DMF and mixed solution c is 6:70-80:20, and the mass ratio of tetrabutylammonium bromide, DL-lipoic acid and anhydrous DMF in the mixed solution c is 0.3:3-4:10. In the above process, with tetrabutylammonium bromide as a catalyst, the epoxy group on the epoxy nano-silica and the carboxyl group on the DL-lipoic acid undergo a ring-opening reaction to obtain modified nano-silica;

[0033] Step C3, adding modified nano-silica and L-hydroxyproline to anhydrous DMF, stirring evenly, then adding p-toluenesulfonic acid, heating to 65-75°C, continuing to stir and react for 4.5-5.5h, filtering after the reaction, washing and drying the filter cake to obtain functionalized nano-silica, wherein the mass ratio of modified nano-silica, L-hydroxyproline, anhydrous DMF and p-toluenesulfonic acid is 5:1-2:75-85:0.06-0.08. In the above process, anhydrous DMF is used as solvent and p-toluenesulfonic acid is used as catalyst, and the modified nano-silica and L-hydroxyproline undergo esterification reaction to obtain functionalized nano-silica.

[0034] In summary, the present application has the following beneficial effects: in order to improve the weather resistance, fire resistance and moisture resistance of the plugging composite material, the present invention starts from two aspects. First, a toughening and repairing component is added to the plugging composite material. The outer layer of the toughening and repairing component is a polyhydroxy monomer structure obtained by chemically crosslinking dihydroxy phosphate and terminal carboxyl polybutadiene, and the inner core contains functionalized nano-silica. The functional nano-silica is prepared by KH-560 modified nano-silica, which is further chemically bonded with DL-lipoic acid and finally chemically crosslinked with L-hydroxyproline. The dihydroxy phosphate contains a phosphate group. The presence of the low-polarity phosphate group can, on the one hand, play a synergistic role with the functionalized silica structure, enhance the compatibility of the polybutadiene structure with the epoxy resin, and improve the mechanical properties of the plugging composite material. On the other hand, the phosphate group and the ester group in the functionalized nano-silica can be used as an acid source, the terminal carboxyl polybutadiene can be used as a carbon source, and the amide group and amino group in the functionalized nano-silica can be used as a nitrogen source. They constitute The intumescent flame retardant system improves the fire resistance of the plugging composite material. On the one hand, the amino group in the functionalized nano-silica can chemically cross-link with the epoxy resin in the substrate to improve the cross-linking degree of the system, strengthen the bonding force between molecules, and make it difficult for water molecules to enter the interior of the molecule through the coating film, thereby improving the moisture resistance of the plugging composite material. On the other hand, it forms hydrogen bonds with the hydroxyl groups in the functionalized nano-silica and the hydroxyl groups in the polyhydroxy monomer structure. The disulfide bonds contained in the functionalized nano-silica give the toughening and repairing components self-repairing properties, thereby improving the weather resistance and mechanical properties of the plugging composite material. Second, the addition of weather-resistant components can, on the one hand, exert the UV resistance of the cellulose structure and thus improve the weather resistance of the plugging composite material. On the other hand, the 2-mercaptonicotinic acid grafted on the surface of the weather-resistant component has a mercapto group that can chemically bond with the unsaturated double bonds in the toughening and repairing component. Introducing it into the plugging composite material can work synergistically with the toughening and repairing component to jointly improve the weather resistance, fire resistance, moisture resistance and mechanical properties of the plugging material. DETAILED DESCRIPTION

[0035] The contents of the main raw materials and their components used in the examples are as follows:

[0036] The number average molecular weight of the carboxyl-terminated polybutadiene was 2400, and the carboxyl value was 0.05.

[0037] The present application is further described in detail below in conjunction with embodiments.

[0038] Preparation Examples 1-3 and Comparative Preparation Example 1 provide methods for preparing weather-resistant components.

[0039] Preparation Example 1

[0040] The weather-resistant component is prepared by the following steps:

[0041] Step A1, stirring microcrystalline cellulose and a 62% sulfuric acid solution at a speed of 400 rpm for 30 minutes until uniform, maintaining the speed unchanged, heating to 55°C, stirring for 2 hours, adding deionized water, standing for 4 hours, precipitating, removing the supernatant, centrifuging the remaining suspension, dialyzing through a dialysis bag with a pore size of 120 kDa for 3.5 hours, and freeze-drying at -35°C to constant weight to obtain cellulose nanocrystals, wherein the mass ratio of microcrystalline cellulose, a 62% sulfuric acid solution and deionized water is 1:13:40;

[0042] Step A2, adding cellulose nanocrystals, 2-mercaptonicotinic acid and trifluoromethanesulfonic acid to anhydrous DMF, stirring at a speed of 500 rpm for 40 minutes until uniform, maintaining the speed unchanged, heating to 110°C under nitrogen protection, stirring and reacting for 18 hours, after the reaction is completed, standing for 4 hours, filtering, and washing the filter cake with anhydrous ethanol and deionized water for 3 times in sequence, and drying at 50°C to constant weight to obtain a weather-resistant component, wherein the mass ratio of cellulose nanocrystals, 2-mercaptonicotinic acid, trifluoromethanesulfonic acid and anhydrous DMF is 1:14:0.1:95.

[0043] Preparation Example 2

[0044] The weather-resistant component is prepared by the following steps:

[0045] Step A1, stirring microcrystalline cellulose and a 64% sulfuric acid solution at a speed of 500 rpm for 20 minutes until uniform, maintaining the speed unchanged, heating to 60°C, stirring and reacting for 3 hours, then adding deionized water, standing for 5 hours, precipitating, removing the supernatant, centrifuging the remaining suspension, dialyzing through a dialysis bag with a pore size of 140 kDa for 4.0 hours, and freeze-drying at -40°C to constant weight to obtain cellulose nanocrystals, wherein the mass ratio of microcrystalline cellulose, the 64% sulfuric acid solution and deionized water is 1:14:50;

[0046] Step A2, adding cellulose nanocrystals, 2-mercaptonicotinic acid and trifluoromethanesulfonic acid to anhydrous DMF, stirring at a rotation speed of 550 rpm for 35 minutes until uniform, maintaining the rotation speed unchanged, heating to 100°C under nitrogen protection, stirring and reacting for 19 hours, after the reaction is completed, standing for 5 hours, filtering, and washing the filter cake with anhydrous ethanol and deionized water for 4 times in sequence, and drying at 55°C to constant weight to obtain a weather-resistant component, wherein the mass ratio of cellulose nanocrystals, 2-mercaptonicotinic acid and trifluoromethanesulfonic acid to anhydrous DMF is 1:15:0.15:100.

[0047] Preparation Example 3

[0048] The weather-resistant component is prepared by the following steps:

[0049] Step A1, stirring microcrystalline cellulose and a 66% sulfuric acid solution at a rotation speed of 600 rpm for 10 min until uniform, maintaining the rotation speed unchanged, heating to 65°C, stirring and reacting for 4 h, then adding deionized water, standing for 6 h, precipitating, removing the supernatant, centrifuging the remaining suspension, dialyzing through a dialysis bag with a pore size of 160 kDa for 4.5 h, and freeze-drying at -45°C to constant weight to obtain cellulose nanocrystals, wherein the mass ratio of microcrystalline cellulose, a 66% sulfuric acid solution and deionized water is 1:15:60;

[0050] Step A2, adding cellulose nanocrystals, 2-mercaptonicotinic acid and trifluoromethanesulfonic acid to anhydrous DMF, stirring at a speed of 600 rpm for 30 minutes until uniform, maintaining the speed unchanged, heating to 90°C under nitrogen protection, stirring and reacting for 18 hours, after the reaction is completed, standing for 6 hours, filtering, and washing the filter cake with anhydrous ethanol and deionized water for 5 times in sequence, and drying at 60°C to constant weight to obtain a weather-resistant component, wherein the mass ratio of cellulose nanocrystals, 2-mercaptonicotinic acid, trifluoromethanesulfonic acid and anhydrous DMF is 1:16:0.2:105.

[0051] Comparative Preparation Example 1

[0052] The weather-resistant component is prepared by the following steps:

[0053] Step A1, stirring microcrystalline cellulose and a 62% sulfuric acid solution at a speed of 400 rpm for 30 minutes until uniform, maintaining the speed unchanged, heating to 55°C, stirring for reaction for 2 hours, adding deionized water, standing for 4 hours, precipitating, removing the supernatant, centrifuging the remaining suspension, dialyzing through a dialysis bag with a pore size of 120 kDa for 3.5 hours, and freeze-drying at -35°C to constant weight to obtain cellulose nanocrystals, wherein the mass ratio of microcrystalline cellulose, the 62% sulfuric acid solution and deionized water is 1:13:40;

[0054] Step A2, add cellulose nanocrystals, nicotinic acid and trifluoromethanesulfonic acid to anhydrous DMF, stir at a speed of 500 rpm for 40 minutes until uniform, maintain the speed unchanged, heat to 110°C under nitrogen protection, stir and react for 18 hours, after the reaction is completed, let it stand for 4 hours, filter, wash the filter cake with anhydrous ethanol and deionized water for 3 times, dry at 50°C to constant weight, and obtain a weather-resistant component, wherein the mass ratio of cellulose nanocrystals, nicotinic acid, trifluoromethanesulfonic acid and anhydrous DMF is 1:14:0.1:95.

[0055] Preparation Examples 4-6 and Comparative Preparation Example 2 provide methods for preparing functionalized nano-silicon dioxide.

[0056] Preparation Example 4

[0057] Functionalized nano-silica is prepared by the following steps:

[0058] Step C1, placing the nano-silica in a vacuum drying oven at 80°C and drying for 24 hours, then placing it in a mixed solution a of anhydrous ethanol and deionized water, controlling the ultrasonic power to 300W for 0.5 hours, and stirring at a speed of 500rpm for 30 minutes until uniform, and when the temperature is constant and the speed is maintained unchanged, adding a mixed solution b of KH-560 and anhydrous ethanol, and controlling the dripping to be completed within 10 minutes, after the dripping is completed, heating to 60°C, stirring and reacting for 4 hours, cooling to room temperature after the reaction, centrifuging, and then washing with anhydrous ethanol and deionized water three times in sequence, and vacuum drying at 55°C to constant weight to obtain epoxy nano-silica, wherein the mass ratio of nano-silica, mixed solution a and mixed solution b is 5:40:12, the mass ratio of anhydrous ethanol and deionized water in the mixed solution a is 20:10, and the mass ratio of KH-560 and anhydrous ethanol in the mixed solution b is 0.3:10;

[0059] Step C2, adding epoxy nano-silica to anhydrous DMF, controlling the speed to 500 rpm and stirring for 30 minutes until uniform, maintaining the speed unchanged, adding tetrabutylammonium bromide, DL-lipoic acid and anhydrous DMF mixed solution c dropwise while stirring, controlling the dripping to be completed within 30 minutes, raising the temperature to 105°C, stirring and reacting for 2 hours, centrifuging after the reaction, washing the precipitate with anhydrous ethanol and deionized water for 3 times, and drying at 55°C to constant weight to obtain modified nano-silica, wherein the mass ratio of epoxy nano-silica, anhydrous DMF and mixed solution c is 6:70:20, and the mass ratio of tetrabutylammonium bromide, DL-lipoic acid and anhydrous DMF in the mixed solution c is 0.3:3:10;

[0060] Step C3, adding modified nano-silica and L-hydroxyproline to anhydrous DMF, controlling the speed to 550 rpm and stirring for 35 minutes until uniform, maintaining the speed unchanged, then adding p-toluenesulfonic acid, raising the temperature to 65°C, continuing to stir and react for 4.5 hours, after the reaction is completed, filtering, washing the filter cake with a mass fraction of 40% ethanol aqueous solution for 3 times, and drying at 40°C to constant weight to obtain functionalized nano-silica, wherein the mass ratio of modified nano-silica, L-hydroxyproline, anhydrous DMF and p-toluenesulfonic acid is 5:1:75:0.06.

[0061] Preparation Example 5

[0062] Functionalized nano-silica is prepared by the following steps:

[0063] Step C1, placing the nano-silica in a vacuum drying oven at 80°C and drying for 24 hours, then placing it in a mixture of anhydrous ethanol and deionized water a, controlling the ultrasonic power to 350W for 0.75 hours, and stirring at a speed of 550rpm for 25 minutes until uniform, and when the temperature is constant and the speed is maintained unchanged, adding a mixture of KH-560 and anhydrous ethanol b dropwise, and controlling the dripping to be completed within 10 minutes, after the dripping is completed, heating to 65°C, stirring and reacting for 5 hours, cooling to room temperature after the reaction is completed, centrifuging, and then washing with anhydrous ethanol and deionized water for 4 times in turn, and vacuum drying at 60°C to constant weight to obtain epoxy nano-silica, wherein the mass ratio of nano-silica, mixture a and mixture b is 5:45:13, the mass ratio of anhydrous ethanol and deionized water in the mixture a is 22:10, and the mass ratio of KH-560 and anhydrous ethanol in the mixture b is 0.4:10;

[0064] Step C2, adding epoxy nano-silica to anhydrous DMF, controlling the speed to 600 rpm and stirring for 25 minutes until uniform, maintaining the speed unchanged, adding tetrabutylammonium bromide, DL-lipoic acid and anhydrous DMF mixed solution c dropwise while stirring, controlling the dripping to be completed within 30 minutes, raising the temperature to 110°C, stirring and reacting for 2.5 hours, centrifuging after the reaction, washing the precipitate with anhydrous ethanol and deionized water for 4 times, and drying at 65°C to constant weight to obtain modified nano-silica, wherein the mass ratio of epoxy nano-silica, anhydrous DMF and mixed solution c is 6:75:20, and the mass ratio of tetrabutylammonium bromide, DL-lipoic acid and anhydrous DMF in the mixed solution c is 0.3:3.5:10;

[0065] Step C3, adding modified nano-silica and L-hydroxyproline to anhydrous DMF, controlling the speed to 600 rpm and stirring for 30 minutes until uniform, maintaining the speed unchanged, then adding p-toluenesulfonic acid, heating to 70°C, continuing to stir and react for 5.0 hours, after the reaction is completed, filtering, washing the filter cake with a mass fraction of 40% ethanol aqueous solution 4 times, and drying at 45°C to constant weight to obtain functionalized nano-silica, wherein the mass ratio of modified nano-silica, L-hydroxyproline, anhydrous DMF and p-toluenesulfonic acid is 5:1.5:80:0.07.

[0066] Preparation Example 6

[0067] Functionalized nano-silica is prepared by the following steps:

[0068] Step C1, placing the nano-silica in a vacuum drying oven at 80°C and drying for 24 hours, then placing it in a mixed solution a of anhydrous ethanol and deionized water, controlling the ultrasonic power to 400W for 1 hour, and stirring at a speed of 600rpm for 20 minutes until uniform, and when the temperature is constant and the speed is maintained unchanged, adding a mixed solution b of KH-560 and anhydrous ethanol, and controlling the dripping to be completed within 10 minutes, after the dripping is completed, heating to 70°C, stirring and reacting for 6 hours, cooling to room temperature after the reaction, centrifuging, and then washing with anhydrous ethanol and deionized water for 5 times in sequence, and vacuum drying at 65°C to constant weight to obtain epoxy nano-silica, wherein the mass ratio of nano-silica, mixed solution a and mixed solution b is 5:50:14, the mass ratio of anhydrous ethanol and deionized water in the mixed solution a is 24:10, and the mass ratio of KH-560 and anhydrous ethanol in the mixed solution b is 0.5:10;

[0069] Step C2, adding epoxy nano-silica to anhydrous DMF, controlling the speed to 700 rpm and stirring for 20 minutes until uniform, maintaining the speed unchanged, adding tetrabutylammonium bromide, DL-lipoic acid and anhydrous DMF mixed solution c dropwise while stirring, controlling the dripping to be completed within 30 minutes, raising the temperature to 115°C, stirring and reacting for 3 hours, centrifuging after the reaction, washing the precipitate with anhydrous ethanol and deionized water for 5 times, and drying at 70°C to constant weight to obtain modified nano-silica, wherein the mass ratio of epoxy nano-silica, anhydrous DMF and mixed solution c is 6:80:20, and the mass ratio of tetrabutylammonium bromide, DL-lipoic acid and anhydrous DMF in the mixed solution c is 0.3:4:10;

[0070] Step C3, adding modified nano-silica and L-hydroxyproline to anhydrous DMF, controlling the speed to 650 rpm and stirring for 25 minutes until uniform, maintaining the speed unchanged, then adding p-toluenesulfonic acid, raising the temperature to 75°C, continuing to stir and react for 5.5 hours, after the reaction is completed, filtering, washing the filter cake with a mass fraction of 40% ethanol aqueous solution for 5 times, and drying at 50°C to constant weight to obtain functionalized nano-silica, wherein the mass ratio of modified nano-silica, L-hydroxyproline, anhydrous DMF and p-toluenesulfonic acid is 5:2:85:0.08.

[0071] Comparative Preparation Example 2

[0072] Functionalized nano-silica is prepared by the following steps:

[0073] Step C1, placing the nano-silica in a vacuum drying oven at 80°C and drying for 24 hours, then placing it in a mixed solution a of anhydrous ethanol and deionized water, controlling the ultrasonic power to 300W for 0.5 hours, and stirring at a speed of 500rpm for 30 minutes until uniform, and when the temperature is constant and the speed is maintained unchanged, adding a mixed solution b of KH-560 and anhydrous ethanol, and controlling the dripping to be completed within 10 minutes, after the dripping is completed, heating to 60°C, stirring and reacting for 4 hours, cooling to room temperature after the reaction, centrifuging, and then washing with anhydrous ethanol and deionized water three times in sequence, and vacuum drying at 55°C to constant weight to obtain epoxy nano-silica, wherein the mass ratio of nano-silica, mixed solution a and mixed solution b is 5:40:12, the mass ratio of anhydrous ethanol and deionized water in the mixed solution a is 20:10, and the mass ratio of KH-560 and anhydrous ethanol in the mixed solution b is 0.3:10;

[0074] Step C2, adding epoxy nano-silica to anhydrous DMF, controlling the speed to 500 rpm and stirring for 30 minutes until uniform, maintaining the speed unchanged, adding tetrabutylammonium bromide, octanoic acid and anhydrous DMF mixed solution c dropwise while stirring, controlling the dripping to be completed within 30 minutes, raising the temperature to 105°C, stirring and reacting for 2 hours, centrifuging after the reaction, washing the precipitate with anhydrous ethanol and deionized water for 3 times, and drying at 55°C to constant weight to obtain modified nano-silica, wherein the mass ratio of epoxy nano-silica, anhydrous DMF and mixed solution c is 6:70:20, and the mass ratio of tetrabutylammonium bromide, octanoic acid and anhydrous DMF in the mixed solution c is 0.3:3:10;

[0075] Step C3, add modified nano-silica and L-hydroxyproline to anhydrous DMF, control the speed to 550 rpm and stir for 35 minutes until uniform, maintain the speed unchanged, then add p-toluenesulfonic acid, raise the temperature to 65°C, continue stirring and react for 4.5 hours, after the reaction is completed, filter, wash the filter cake with 40% ethanol aqueous solution by mass fraction 3 times, and dry it at 40°C to constant weight, to obtain functionalized nano-silica modified nano-silica, L-hydroxyproline, anhydrous DMF and p-toluenesulfonic acid The mass ratio is 5:1:75:0.06.

[0076] Preparation Examples 7-9 and Comparative Preparation Examples 3-4 provide methods for preparing toughening repair components.

[0077] Preparation Example 7

[0078] The toughening and repairing component is prepared by the following steps:

[0079] Step B1, stirring carbon tetrachloride and tetrahydrofuran at a speed of 500 rpm for 30 min, adding dibutyl phosphite, and then adding triethylamine and ethanolamine in an ice-water bath, maintaining the speed unchanged, heating to 45°C, continuing to stir and react for 8 hours, filtering with suction, and rotary evaporating the filtrate at 60°C to constant weight to obtain dihydroxy phosphate, wherein the mass ratio of carbon tetrachloride, tetrahydrofuran, dibutyl phosphite, triethylamine and ethanolamine is 70:35:4:1.5:2.2;

[0080] Step B2, under nitrogen protection, add terminal carboxyl polybutadiene and dihydroxy phosphate to tetrahydrofuran, control the speed to 700 rpm and stir for 25 minutes until uniform, then add dicyclohexylcarbodiimide and 4-dimethylaminopyridine, maintain the speed unchanged, raise the temperature to reflux, stir and react for 4 hours, after the reaction is completed, cool to room temperature, filter, wash the filter cake with anhydrous ethanol and deionized water for 3 times, freeze-dry at -30°C to constant weight, and obtain a polyhydroxy monomer, wherein the mass ratio of terminal carboxyl polybutadiene, dihydroxy phosphate, tetrahydrofuran, dicyclohexylcarbodiimide and 4-dimethylaminopyridine is 1:2.4:30:2.3:1.4;

[0081] Step B3, add the polyhydroxy monomer and the functionalized nano-silica prepared in Preparation Example 4 to anhydrous toluene, control the speed to stir for 2 hours at 300 rpm, filter, and dry to constant weight at 50°C to obtain a toughening and repair component, wherein the mass ratio of the polyhydroxy monomer, the functionalized nano-silica prepared in Preparation Example 4 and anhydrous toluene is 12:1:60.

[0082] Preparation Example 8

[0083] The toughening and repairing component is prepared by the following steps:

[0084] Step B1, stirring carbon tetrachloride and tetrahydrofuran at a speed of 600 rpm for 25 min, adding dibutyl phosphite, and then adding triethylamine and ethanolamine in an ice-water bath, heating to 50° C., maintaining the speed unchanged, stirring and reacting for 9 h, filtering with suction, and rotary evaporating the filtrate at 65° C. to constant weight to obtain dihydroxy phosphate, wherein the mass ratio of carbon tetrachloride, tetrahydrofuran, dibutyl phosphite, triethylamine and ethanolamine is 75:40:5:1.8:2.7;

[0085] Step B2, under nitrogen protection, add terminal carboxyl polybutadiene and dihydroxy phosphate to tetrahydrofuran, control the speed to 650 rpm and stir for 30 minutes until uniform, then add dicyclohexylcarbodiimide and 4-dimethylaminopyridine, maintain the speed unchanged, raise the temperature to reflux, stir and react for 5 hours, after the reaction is completed, cool to room temperature, filter, wash the filter cake with anhydrous ethanol and deionized water for 4 times, freeze-dry at -35°C to constant weight, and obtain a polyhydroxy monomer, wherein the mass ratio of terminal carboxyl polybutadiene, dihydroxy phosphate, tetrahydrofuran, dicyclohexylcarbodiimide and 4-dimethylaminopyridine is 1:2.8:40:2.4:1.6;

[0086] Step B3, add the polyhydroxy monomer and the functionalized nano-silica prepared in Preparation Example 5 to anhydrous toluene, stir for 1.5 hours at a controlled speed of 350 rpm, filter, and dry to constant weight at 55°C to obtain a toughening and repair component, wherein the mass ratio of the polyhydroxy monomer, the functionalized nano-silica prepared in Preparation Example 5 and anhydrous toluene is 14:2:65.

[0087] Preparation Example 9

[0088] The toughening and repairing component is prepared by the following steps:

[0089] Step B1, stirring carbon tetrachloride and tetrahydrofuran at a speed of 700 rpm for 20 min, adding dibutyl phosphite, and then adding triethylamine and ethanolamine under an ice-water bath, heating to 55° C., maintaining the speed unchanged, stirring and reacting for 10 h, filtering with suction, and rotary evaporating the filtrate at 70° C. to constant weight to obtain dihydroxy phosphate, wherein the mass ratio of carbon tetrachloride, tetrahydrofuran, dibutyl phosphite, triethylamine and ethanolamine is 80:45:6:2.1:3.2;

[0090] Step B2, under nitrogen protection, add terminal carboxyl polybutadiene and dihydroxy phosphate to tetrahydrofuran, control the speed to 600 rpm and stir for 35 minutes until uniform, then add dicyclohexylcarbodiimide and 4-dimethylaminopyridine, maintain the speed unchanged, raise the temperature to reflux, stir and react for 6 hours, after the reaction is completed, cool to room temperature, filter, wash the filter cake with anhydrous ethanol and deionized water for 5 times, freeze-dry at -40°C to constant weight, and obtain a polyhydroxy monomer, wherein the mass ratio of terminal carboxyl polybutadiene, dihydroxy phosphate, tetrahydrofuran, dicyclohexylcarbodiimide and 4-dimethylaminopyridine is 1:3.2:50:2.5:1.8;

[0091] Step B3, add the polyhydroxy monomer and the functionalized nano-silica prepared in Preparation Example 6 to anhydrous toluene, stir at a speed of 400 rpm for 1 hour, filter, and dry at 60°C to constant weight to obtain a toughening and repair component, wherein the mass ratio of the polyhydroxy monomer, the functionalized nano-silica prepared in Preparation Example 6 and anhydrous toluene is 16:3:70.

[0092] Comparative Preparation Example 3

[0093] The toughening and repairing component is prepared by the following steps:

[0094] Step B1, stirring carbon tetrachloride and tetrahydrofuran at a speed of 500 rpm for 30 min, adding dibutyl phosphite, and then adding triethylamine and ethanolamine in an ice-water bath, maintaining the speed unchanged, heating to 45°C, continuing to stir and react for 8 hours, filtering with suction, and rotary evaporating the filtrate at 60°C to constant weight to obtain dihydroxy phosphate, wherein the mass ratio of carbon tetrachloride, tetrahydrofuran, dibutyl phosphite, triethylamine and ethanolamine is 70:35:4:1.5:2.2;

[0095] Step B2, under nitrogen protection, add terminal carboxyl polybutadiene and dihydroxy phosphate to tetrahydrofuran, control the speed to 700 rpm and stir for 25 minutes until uniform, then add dicyclohexylcarbodiimide and 4-dimethylaminopyridine, maintain the speed unchanged, raise the temperature to reflux, stir and react for 4 hours, after the reaction is completed, cool to room temperature, filter, wash the filter cake with anhydrous ethanol and deionized water for 3 times, freeze-dry at -30°C to constant weight, and obtain a polyhydroxy monomer, wherein the mass ratio of terminal carboxyl polybutadiene, dihydroxy phosphate, tetrahydrofuran, dicyclohexylcarbodiimide and 4-dimethylaminopyridine is 1:2.4:30:2.3:1.4;

[0096] Step B3, add the polyhydroxy monomer and the functionalized nano-silica prepared in Comparative Preparation Example 2 to anhydrous toluene, control the speed to stir for 2 hours at 300 rpm, filter, and dry to constant weight at 50°C to obtain a toughening and repair component, wherein the mass ratio of the polyhydroxy monomer, the functionalized nano-silica prepared in Comparative Preparation Example 2 and anhydrous toluene is 12:1:60.

[0097] Comparative Preparation Example 4

[0098] The toughening and repairing component is prepared by the following steps:

[0099] Step B1, stirring carbon tetrachloride and tetrahydrofuran at a speed of 500 rpm for 30 min, adding O-butyl lactylate, and then adding triethylamine and ethanolamine in an ice-water bath, maintaining the speed unchanged, heating to 45°C, continuing to stir and react for 8 hours, filtering with suction, and rotary evaporating the filtrate at 60°C to constant weight to obtain dihydroxy phosphate, wherein the mass ratio of carbon tetrachloride, tetrahydrofuran, O-butyl lactylate, triethylamine and ethanolamine is 70:35:4:1.5:2.2;

[0100] Step B2, under nitrogen protection, add terminal carboxyl polybutadiene and dihydroxy phosphate to tetrahydrofuran, control the speed to 700 rpm and stir for 25 minutes until uniform, then add dicyclohexylcarbodiimide and 4-dimethylaminopyridine, maintain the speed unchanged, raise the temperature to reflux, stir and react for 4 hours, after the reaction is completed, cool to room temperature, filter, wash the filter cake with anhydrous ethanol and deionized water for 3 times, freeze-dry at -30°C to constant weight, and obtain a polyhydroxy monomer, wherein the mass ratio of terminal carboxyl polybutadiene, dihydroxy phosphate, tetrahydrofuran, dicyclohexylcarbodiimide and 4-dimethylaminopyridine is 1:2.4:30:2.3:1.4;

[0101] Step B3, add the polyhydroxy monomer and the functionalized nano-silica prepared in Preparation Example 4 to anhydrous toluene, control the speed to stir for 2 hours at 300 rpm, filter, and dry to constant weight at 50°C to obtain a toughening and repair component, wherein the mass ratio of the polyhydroxy monomer, the functionalized nano-silica prepared in Preparation Example 4 and anhydrous toluene is 12:1:60.

[0102] Examples 1-3 and Comparative Examples 1-3 provide polymer moisture-proof and fire-proof sealing composite materials and preparation methods thereof. Example 1

[0103] The present embodiment provides a polymer moisture-proof and fire-proof sealing composite material, comprising the following raw materials in parts by weight: 55 parts of bisphenol A epoxy resin, 8 parts of the weather-resistant component prepared in Preparation Example 1, 12 parts of the toughening and repairing component prepared in Preparation Example 7, 5 parts of ethylene glycol diglycidyl ether, 2 parts of polyether silicone oil JF-956, 1.2 parts of accelerator K-54, 16 parts of polyether amine D230 and 0.6 parts of benzoin dimethyl ether;

[0104] The preparation method of the polymer moisture-proof and fire-proof sealing composite material comprises the following steps:

[0105] Step S1, stirring bisphenol A epoxy resin, toughening and repairing component, ethylene glycol diglycidyl ether and polyether silicone oil JF-956 at a speed of 700 rpm for 20 minutes, and vacuum degassing to obtain component A;

[0106] Step S2, stirring the weather-resistant component, accelerator K-54, polyetheramine D230 and benzoin dimethyl ether at a rotation speed of 600 rpm for 30 minutes to prepare component B;

[0107] Step S3, encapsulating the combination A and the component B separately to obtain a polymer moisture-proof and fire-proof sealing composite material. Example 2

[0108] The present embodiment provides a polymer moisture-proof and fire-proof sealing composite material, comprising the following raw materials in parts by weight: 62.5 parts of bisphenol F epoxy resin, 9 parts of weather-resistant component prepared in Preparation Example 2, 14 parts of toughening and repair component prepared in Preparation Example 8, 7.5 parts of ethylene glycol diglycidyl ether, 3.5 parts of polyether silicone oil JF-956, 1.35 parts of accelerator K-54, 17 parts of polyether amine D230 and 0.7 parts of benzoin dimethyl ether;

[0109] The preparation method of the polymer moisture-proof and fire-proof sealing composite material comprises the following steps:

[0110] Step S1, stirring bisphenol F epoxy resin, toughening and repairing component, ethylene glycol diglycidyl ether and polyether silicone oil JF-956 at a speed of 600 rpm for 30 minutes, and vacuum degassing to obtain component A;

[0111] Step S2, stirring the weather-resistant component, accelerator K-54, polyetheramine D230 and benzoin dimethyl ether at a rotation speed of 500 rpm for 40 minutes to prepare component B;

[0112] Step S3, encapsulating the combination A and the component B separately to obtain a polymer moisture-proof and fire-proof sealing composite material. Example 3

[0113] The present embodiment provides a polymer moisture-proof and fire-proof sealing composite material, comprising the following raw materials in parts by weight: 70 parts of bisphenol A epoxy resin, 10 parts of the weather-resistant component prepared in Preparation Example 3, 16 parts of the toughening and repairing component prepared in Preparation Example 9, 10 parts of ethylene glycol diglycidyl ether, 5 parts of polyether silicone oil JF-956, 1.5 parts of accelerator K-54, 18 parts of polyether amine D230 and 0.8 parts of benzoin dimethyl ether;

[0114] The preparation method of the polymer moisture-proof and fire-proof sealing composite material comprises the following steps:

[0115] Step S1, stirring bisphenol A epoxy resin, toughening and repairing component, ethylene glycol diglycidyl ether and polyether silicone oil JF-956 at a speed of 500 rpm for 40 minutes, and vacuum degassing to obtain component A;

[0116] Step S2, stirring the weather-resistant component, accelerator K-54, polyetheramine D23 and benzoin dimethyl ether at a rotation speed of 400 rpm for 50 minutes to prepare component B;

[0117] Step S3, encapsulating the combination A and the component B separately to obtain a polymer moisture-proof and fire-proof sealing composite material. Comparative Example 1

[0118] This comparative example provides a polymer moisture-proof and fire-proof sealing composite material, comprising the following raw materials in parts by weight: 55 parts of bisphenol A epoxy resin, 8 parts of weather-resistant components prepared in comparative preparation example 1, 12 parts of toughening and repair components prepared in preparation example 7, 5 parts of ethylene glycol diglycidyl ether, 2 parts of polyether silicone oil JF-956, 1.2 parts of accelerator K-54, 16 parts of polyether amine D230 and 0.6 parts of benzoin dimethyl ether;

[0119] The preparation method of the polymer moisture-proof and fire-proof sealing composite material comprises the following steps:

[0120] Step S1, stirring bisphenol A epoxy resin, toughening and repairing component, ethylene glycol diglycidyl ether and polyether silicone oil JF-956 at a speed of 700 rpm for 20 minutes, and vacuum degassing to obtain component A;

[0121] Step S2, stirring the weather-resistant component, accelerator K-54, polyetheramine D230 and benzoin dimethyl ether at a rotation speed of 600 rpm for 30 minutes to prepare component B;

[0122] Step S3, encapsulating the combination A and the component B separately to obtain a polymer moisture-proof and fire-proof sealing composite material. Comparative Example 2

[0123] This comparative example provides a polymer moisture-proof and fire-proof sealing composite material, comprising the following raw materials in parts by weight: 55 parts of bisphenol A epoxy resin, 8 parts of weather-resistant components prepared in Preparation Example 1, 12 parts of toughening and repair components prepared in Comparative Preparation Example 3, 5 parts of ethylene glycol diglycidyl ether, 2 parts of polyether silicone oil JF-956, 1.2 parts of accelerator K-54, 16 parts of polyether amine D230 and 0.6 parts of benzoin dimethyl ether;

[0124] The preparation method of the polymer moisture-proof and fire-proof sealing composite material comprises the following steps:

[0125] Step S1, stirring bisphenol A epoxy resin, toughening and repairing component, ethylene glycol diglycidyl ether and polyether silicone oil JF-956 at a speed of 700 rpm for 20 minutes, and vacuum degassing to obtain component A;

[0126] Step S2, stirring the weather-resistant component, accelerator K-54, polyetheramine D230 and benzoin dimethyl ether at a rotation speed of 600 rpm for 30 minutes to prepare component B;

[0127] Step S3, encapsulating the combination A and the component B separately to obtain a polymer moisture-proof and fire-proof sealing composite material. Comparative Example 3

[0128] This comparative example provides a polymer moisture-proof and fire-proof sealing composite material, comprising the following raw materials in parts by weight: 55 parts of bisphenol A epoxy resin, 8 parts of weather-resistant components prepared in Preparation Example 1, 12 parts of toughening and repair components prepared in Comparative Preparation Example 4, 5 parts of ethylene glycol diglycidyl ether, 2 parts of polyether silicone oil JF-956, 1.2 parts of accelerator K-54, 16 parts of polyether amine D230 and 0.6 parts of benzoin dimethyl ether;

[0129] The preparation method of the polymer moisture-proof and fire-proof sealing composite material comprises the following steps:

[0130] Step S1, stirring bisphenol A epoxy resin, toughening and repairing component, ethylene glycol diglycidyl ether and polyether silicone oil JF-956 at a speed of 700 rpm for 20 minutes, and vacuum degassing to obtain component A;

[0131] Step S2, stirring the weather-resistant component, accelerator K-54, polyetheramine D230 and benzoin dimethyl ether at a rotation speed of 600 rpm for 30 minutes to prepare component B;

[0132] Step S3, encapsulating the combination A and the component B separately to obtain a polymer moisture-proof and fire-proof sealing composite material.

[0133] Performance Testing

[0134] Preparation of test samples

[0135] Component A and component B in the polymer moisture-proof and fire-proof plugging composite materials prepared in Examples 1-3 and Comparative Examples 1-3 were stirred at a speed of 500 rpm for 30 min until uniform, then poured onto a clean polytetrafluoroethylene plate, and coated with a four-sided film applicator from 100 μm, 200 μm, 300 μm to 600 μm in sequence, and then placed at a wavelength peak of 365 nm and an intensity of 80 mw / cm 2 The film was irradiated under ultraviolet light for 15 min, the irradiation temperature was controlled at 60°C, and then dried and cured at room temperature for 24 h. Then, the film was cured at 23°C and 50% humidity for 7 h. A scraper was used to separate the membrane and the polytetrafluoroethylene plate to obtain a test sample.

[0136] 1. Fire performance testing

[0137] The test samples prepared in Examples 1-3 and Comparative Examples 1-3 were tested for limiting oxygen index according to GB / T8626-2007. The test results are shown in Table 1.

[0138] Table 1 Fireproof performance test data of polymer moisture-proof and fireproof plugging composite materials prepared in Examples 1-3 and Comparative Examples 1-3

[0139]

[0140] It can be seen from Table 1 that, compared with Comparative Examples 1-3, the oxygen index of the plugging composite materials prepared in Examples 1-3 is higher. Therefore, the plugging composite materials prepared in the present invention have excellent fireproof performance.

[0141] 2. Mechanical properties test

[0142] The mechanical properties of the moisture-proof and fire-proof sealing composite materials prepared in Examples 1-3 and Comparative Examples 1-3, namely, tensile modulus, tensile strength and elongation at break, were tested in sequence using the ASTM D882-12 material testing system;

[0143] Adhesion test: According to the standard ASTMD 4541, the prepared moisture-proof and fire-proof sealing composite material is 2 The amount of the coating was applied on the steel plate. The material of the steel plate conformed to the standard GB / T9271. After sandblasting, the rust removal level reached the Sa2.5 level specified in GB / T8923, and the surface roughness reached the intermediate level specified in GB / T13288.1. After curing for 7 days at 23±2℃ and 50±5% humidity, the test was carried out.

[0144] Pencil hardness: Referring to the national standard GB / 6739-1996 "Pencil Determination of Coating Hardness", the wooden part of the test pencil is shaved off to expose the pencil lead of about 3mm, and the pencil lead is ground into a plane by drawing circles on 400# sandpaper vertically until the edge is sharp. The pencil is scratched on the coating film at an angle of 45° for about 1cm, and the number of pencils that are not scratched is used to indicate the hardness; the test results of Examples 1-3 and Comparative Examples 1-3 are shown in Table 2:

[0145] Table 2 Mechanical properties test data of polymer moisture-proof and fire-proof plugging composite materials prepared in Examples 1-3 and Comparative Examples 1-3

[0146]

[0147] It can be seen from Table 2 that, compared with Comparative Examples 1-3, the plugging composite materials prepared in Examples 1-3 have higher tensile strength and impact resistance and better adhesion performance. Therefore, the plugging composite materials prepared in the present invention have excellent mechanical properties.

[0148] 3. Test the acid resistance, alkali resistance, salt resistance and aging resistance of the samples. The specific technical indicators and test methods are shown in Table 3 below:

[0149] Table 3 Specific technical indicators and test methods for acid resistance, alkali resistance, salt resistance and aging resistance tests

[0150]

[0151] Table 4 Test data of acid resistance, alkali resistance, salt resistance and aging resistance of polymer moisture-proof and fire-proof plugging composite materials prepared in Examples 1-3 and Comparative Examples 1-3

[0152]

[0153] It can be seen from Table 4 that, compared with Comparative Examples 1-3, the aging resistance of the plugging composite material prepared in Examples 1-3 is greater than 1800 h, and no blistering, whitening or cracking will occur when immersed in acid solution, alkali solution and salt solution. Therefore, the plugging composite material prepared by the present invention has more excellent weather resistance.

[0154] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A polymer moisture-proof and fire-proof sealing composite material, characterized in that: It includes the following raw materials in parts by weight: 55-70 parts of base epoxy resin, 8-10 parts of weathering component, 12-16 parts of toughening and repairing component, 5-10 parts of diluent, 2-5 parts of leveling agent, 1.2-1.5 parts of accelerator, 16-18 parts of curing agent and 0.6-0.8 parts of photoinitiator; The toughening and repairing component is prepared by chemically bonding dibutyl phosphite and ethanolamine to obtain dihydroxy phosphate, which is then chemically bonded with terminal carboxyl polybutadiene to obtain a polyhydroxy monomer, and finally coated with functionalized nano-silicon dioxide. The functionalized nano-silica is first prepared by modifying nano-silica with KH-560 to obtain epoxy nano-silica, which is then chemically bonded with DL-lipoic acid to obtain modified nano-silica, and finally chemically bonded with L-hydroxyproline to obtain the functionalized nano-silica. The weather-resistant component is firstly prepared by subjecting microcrystalline cellulose to acidification to obtain cellulose nanocrystals, and then chemically bonding with 2-mercaptonicotinic acid.

2. A polymer moisture-proof and fire-proof plugging composite material according to claim 1, characterized in that: The weather-resistant component is prepared by the following steps: Step A1, mixing microcrystalline cellulose and sulfuric acid solution evenly, maintaining the rotation speed unchanged, heating to 55-65°C, stirring for reaction for 2-4 hours, then adding deionized water, standing for 4-6 hours, precipitating, removing the supernatant, centrifuging the remaining suspension, dialyzing, and freeze-drying to obtain cellulose nanocrystals, wherein the mass ratio of microcrystalline cellulose, sulfuric acid solution and deionized water is 1:13-15:40-60; Step A2, adding cellulose nanocrystals, 2-mercaptonicotinic acid and trifluoromethanesulfonic acid to anhydrous DMF, stirring evenly, heating to 90-110° C. and stirring for reaction for 18-20 hours under nitrogen protection, standing for 4-6 hours after the reaction, filtering, washing the filter cake, and drying to obtain a weather-resistant component, wherein the mass ratio of cellulose nanocrystals, 2-mercaptonicotinic acid, trifluoromethanesulfonic acid and anhydrous DMF is 1:14-16:0.1-0.2:95-105.

3. A polymer moisture-proof and fire-proof sealing composite material according to claim 2, characterized in that: In the step A1, the mass fraction of the sulfuric acid solution is 62-66%.

4. A polymer moisture-proof and fire-proof plugging composite material according to claim 2, characterized in that: The dialysis bag used in the dialysis process has a pore size of 120-160 kDa, and the dialysis time is 3.5-4.5 hours.

5. The polymer moisture-proof and fire-proof sealing composite material according to claim 1, characterized in that: The toughening and repairing component is prepared by the following steps: Step B1, mix carbon tetrachloride and tetrahydrofuran evenly, add dibutyl phosphite, add triethylamine and ethanolamine under ice water bath, heat to 45-55°C, stir to react for 8-10h, filter with suction, and rotary evaporate the filtrate to obtain dihydroxy phosphate, wherein the mass ratio of carbon tetrachloride, tetrahydrofuran, dibutyl phosphite, triethylamine and ethanolamine is 70-80:35-45:4-6:1.5-2.1:2.2-3.2; Step B2, under nitrogen protection, add terminal carboxyl polybutadiene and dihydroxy phosphate to tetrahydrofuran, stir evenly, then add dicyclohexylcarbodiimide and 4-dimethylaminopyridine, raise the temperature to reflux, stir and react for 4-6 hours, after the reaction is completed, cool to room temperature, filter with suction, wash the filter cake, freeze-dry, and obtain a polyhydroxy monomer, wherein the mass ratio of terminal carboxyl polybutadiene, dihydroxy phosphate, tetrahydrofuran, dicyclohexylcarbodiimide and 4-dimethylaminopyridine is 1:2.4-3.2:30-50:2.3-2.5:1.4-1.8; Step B3, adding polyhydroxy monomer and functionalized nano-silica into anhydrous toluene, stirring and reacting for 1-2 hours, filtering, and drying to obtain a toughening and repairing component, wherein the mass ratio of polyhydroxy monomer, functionalized nano-silica and anhydrous toluene is 12-16:1-3:60-70.

6. A polymer moisture-proof and fire-proof plugging composite material according to claim 5, characterized in that: The number average molecular weight of the carboxyl-terminated polybutadiene is 2200-2600, and the carboxyl value is 0.04-0.

06.

7. The polymer moisture-proof and fire-proof sealing composite material according to claim 5, characterized in that: The functionalized nano-silicon dioxide is prepared by the following steps: Step C1, placing the nano-silica in a vacuum drying oven at 80°C and drying for 24 hours, then placing it in a mixed solution a of anhydrous ethanol and deionized water, ultrasonically crushing it for 0.5-1 hour, stirring it evenly, and when the temperature is constant, adding a mixed solution b of KH-560 and anhydrous ethanol dropwise, heating it to 60-70°C, stirring and reacting it for 4-6 hours, and cooling it to room temperature after the reaction is completed, centrifuging, washing, and drying to obtain epoxy nano-silica, wherein the mass ratio of the nano-silica, the mixed solution a, and the mixed solution b is 5:40-50:12-14; Step C2, adding epoxy nano-silica to anhydrous DMF, stirring evenly, adding tetrabutylammonium bromide, DL-lipoic acid and a mixed solution c of anhydrous DMF dropwise while stirring, heating to 105-115°C after the addition is completed, stirring and reacting for 2-3 hours, centrifuging after the reaction is completed, washing the precipitate, and drying to obtain modified nano-silica, wherein the mass ratio of epoxy nano-silica, anhydrous DMF and the mixed solution c is 6:70-80:20; Step C3, adding modified nano-silica and L-hydroxyproline to anhydrous DMF, stirring evenly, then adding p-toluenesulfonic acid, heating to 65-75°C, continuing to stir and react for 4.5-5.5 hours, filtering after the reaction, washing and drying the filter cake to obtain functionalized nano-silica, wherein the mass ratio of modified nano-silica, L-hydroxyproline, anhydrous DMF and p-toluenesulfonic acid is 5:1-2:75-85:0.06-0.

08.

8. The polymer moisture-proof and fire-proof sealing composite material according to claim 7, characterized in that: In the mixed solution a, the mass ratio of anhydrous ethanol to deionized water is 20-24:10, in the mixed solution b, the mass ratio of KH-560 to anhydrous ethanol is 0.3-0.5:10, and in the mixed solution c, the mass ratio of tetrabutylammonium bromide, DL-lipoic acid and anhydrous DMF is 0.3:3-4:

10.

9. A method for preparing a polymer moisture-proof and fire-proof sealing composite material according to any one of claims 1 to 8, characterized in that: The following steps are involved: Step S1, mixing the base epoxy resin, toughening and repairing component, diluent and leveling agent uniformly, and preparing component A after vacuum degassing; Step S2, uniformly mixing the weather-resistant component, the accelerator, the curing agent and the photoinitiator to prepare component B; Step S3, encapsulating the component A and the component B separately to obtain a polymer moisture-proof and fire-proof sealing composite material.

Citation Information

Patent Citations

  • Weather-resistant medium-temperature cured epoxy resin adhesive and preparation method thereof

    CN111334232A

  • Single-component epoxy resin packaging transparent adhesive tape and application thereof

    CN112280509A