Moisture-curable hot-melt adhesive sheet and method for making the same
By using polyamide resin, epoxy resin and moisture-cured polymer in hot melt adhesive sheets to form an interpenetrating network structure, the bonding failure of hot melt adhesive sheets under hot and cold impact and high-temperature water boiling is solved. The problem has significantly improved its temperature and hydrolysis resistance.
Patent Information
- Application Number
- CN202411099094.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-12
AI Technical Summary
Existing hot melt adhesive sheets are prone to bond failure when hot and cold impact and high-temperature boiling, and lack temperature resistance and hydrolysis resistance.
A hot melt adhesive layer consisting of polyamide resin, epoxy resin, hydrophobic active agent, organic solvent and moisture-curable polymer is used to form an interpenetrating network structure through cross-linking reaction, and a moisture-curable hot melt is prepared by combining the release layer. Adhesive sheet to improve bonding strength and temperature resistance.
The bonding strength is maintained under hot and cold impact and high-temperature boiling conditions, and the temperature resistance and hydrolysis resistance of the hot melt adhesive sheet are significantly improved.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hot melt adhesive products, and in particular to a moisture-curable hot melt adhesive sheet and a manufacturing method thereof. Background Art
[0002] Hot melt adhesive sheet is a film made of thermoplastic polymer. Its physical state changes with temperature within a certain temperature range, while its chemical properties remain unchanged. It is non-toxic and tasteless, and is an environmentally friendly chemical product. When the temperature reaches above the melting point, it is in a molten state, and when it is below the melting point, it turns into a solid state, thereby achieving bonding. Hot melt adhesive sheets are widely used in technical fields such as multi-layer packaging, composite building materials, home appliances and the automotive industry.
[0003] Existing hot-melt adhesive sheets use polymer materials such as polyethylene-vinyl acetate copolymers and polyolefin copolymers as base resins, graft copolymerize polar monomers such as maleic anhydride and silane through processes such as reaction extrusion and co-extrusion, thereby increasing the bonding effect of the base resin on PVC and metals, and are processed into hot-melt adhesive sheets through film-forming technologies such as casting and film blowing. However, in actual use, the bonding effect of hot-melt adhesive sheets is easily subject to bonding failure when subjected to hot and cold shocks and high-temperature boiling. Summary of the invention
[0004] The first technical problem to be solved by the present invention is: to provide a moisture-curable hot-melt adhesive sheet with good temperature resistance and hydrolysis resistance in view of the deficiencies in the prior art.
[0005] To solve the above-mentioned first technical problem, the technical solution of the present invention is:
[0006] A moisture-curable hot-melt adhesive sheet comprises a release layer and a hot-melt adhesive layer arranged in sequence;
[0007] The hot melt adhesive layer is prepared by uniformly mixing polyamide resin, epoxy resin, hydrophobic active agent, organic solvent, crosslinking agent and moisture curing polymer in a weight ratio of 100: (5-20): (3-10): (300-600): (0.1-5): (5-25).
[0008] Preferably, the release layer is a double-sided release film or a double-sided release paper.
[0009] Preferably, the release layer has a thickness of 25 to 150 μm, and the hot melt adhesive layer has a thickness of 25 to 100 μm.
[0010] Preferably, the epoxy resin is one of bisphenol A epoxy resin, bisphenol F epoxy resin or aliphatic epoxy resin.
[0011] Preferably, the epoxy value of the epoxy resin is 400-700 g / eq.
[0012] The hydrophobic active agent is a polyphenylene ether resin containing a reactive group, and the weight average molecular weight of the polyphenylene ether resin is 1000-3000.
[0013] The organic solvent is one or a mixed solution of two or more of ethanol, isopropanol, ethyl acetate, toluene, acetone and butanone.
[0014] The cross-linking agent is one or a mixture of two or more of isocyanate, polyisocyanate, polyamine and glycidyl ether.
[0015] The moisture curing polymer is an amorphous-alpha-polyolefin containing siloxane.
[0016] The polyamide resin is prepared by high-temperature condensation reaction of dimer acid and polyamine.
[0017] The second technical problem to be solved by the present invention is: to address the deficiencies of the prior art and to provide a method for preparing a moisture-curable hot-melt adhesive sheet, wherein the obtained moisture-curable hot-melt adhesive sheet has good temperature resistance and hydrolysis resistance.
[0018] To solve the above second technical problem, the technical solution of the present invention is:
[0019] A method for preparing a moisture-curable hot-melt adhesive sheet comprises the following steps:
[0020] S01. Preparation of hot melt adhesive
[0021] The polyamide resin, epoxy resin, hydrophobic active agent and organic solvent are mixed in proportion, stirred at 50-70° C. and 250-350 r / min for 40-70 min, and the hot melt adhesive solution is obtained after the mixture is evenly mixed;
[0022] S02. Preparation of moisture-curable hot-melt adhesive sheet
[0023] A cross-linking agent and a moisture-curable polymer are added to the hot melt adhesive liquid prepared in step S01, stirred and dispersed evenly, and then filtered. After being coated on the release layer by a blade coater or a CED coater and dried completely, a release film is attached and rolled up for aging. After aging, the product is peeled off the release film on the composite and rolled up from the back to obtain a moisture-curable hot melt adhesive sheet.
[0024] Due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0025] 1. The moisture-curable hot-melt adhesive sheet prepared by adding different ratios has excellent bonding strength, and the bonding strength decreases little after hot and cold shock and high-temperature boiling.
[0026] 2. The present invention combines a soluble polyamide resin with an epoxy resin and a low molecular weight polyphenylene ether resin containing reactive groups to react with a cross-linking agent to form an interpenetrating network structure. The hot melt adhesive layer is non-sticky at the initial bonding and the bonding strength is improved after high-temperature hot melting, ensuring that the product has high bonding strength during initial hot pressing to achieve a strong bond. After contacting moisture or water, it chemically solidifies with the siloxane groups in the moisture-curing polymer component. The addition of the moisture-curing polymer can further cross-link to achieve the purpose of post-stage curing, further improve the degree of cross-linking and bonding strength, and improve the temperature resistance and hydrolysis resistance of the moisture-curable hot melt adhesive sheet. DETAILED DESCRIPTION
[0027] The present invention will be further described below in conjunction with the embodiments. Example 1
[0028] S1. Preparation of hot melt adhesive
[0029] 100g of American Kraton 2291 polyamide resin, 10g of Nan Ya epoxy resin 901 (bisphenol A epoxy resin), 5g of Sabic polyphenylene ether resin SA90, and 400g of isopropyl alcohol were added into a reaction kettle, and stirred at 60°C and 300r / min for 60min to dissolve and mix evenly to obtain a hot melt adhesive solution;
[0030] S2. Preparation of moisture-curable hot-melt adhesive sheet
[0031] To the hot melt adhesive solution prepared in S1, add 2 g of Covestro isocyanate N3390 and 10 g of Evonik Vestoplast 206 amorphous-α-polyolefin, stir and disperse evenly, and then filter. Use a blade coater or a CED coater to coat 50 μm hot melt adhesive on a 50 μm PET double-sided release film, attach the release film after drying, and roll it up. After ripening, peel off the release film, and roll it up from the back to obtain a moisture-curable hot melt adhesive sheet. Example 2
[0032] S1. Preparation of hot melt adhesive
[0033] 100g of American Kraton 2291 polyamide resin, 15g of Nan Ya epoxy resin 901 (bisphenol A epoxy resin), 8g of Sabic polyphenylene ether resin SA90, and 500g of organic solvent were added into a reactor, and stirred at 50°C and 250r / min for 70min until the mixture was dissolved and mixed uniformly to obtain a hot melt adhesive solution, wherein the organic solvent was a mixed solvent of xylene and isopropanol, and the mass ratio of the solvent was 1:1;
[0034] S2. Preparation of moisture-curable hot-melt adhesive sheet
[0035] 3 g of glycidyl ether and 15 g of Evonik Vestoplast 206 amorphous-α-polyolefin were added to the hot melt adhesive prepared in S1, and the mixture was stirred and dispersed uniformly and then filtered. A 30 μm thick film was coated on a 100 μm PET double-sided release film using a knife coater or a CED coater. After complete drying, the release film was attached and rolled up. After complete aging, the release film was peeled off and rolled up from the back to obtain a moisture-curable hot melt adhesive sheet. Example 3
[0036] S1. Preparation of hot melt adhesive
[0037] 100g Guangzhou Suning 8620M polyamide resin, 8g Tiantai Chemical BFE170 epoxy resin (bisphenol F epoxy resin), 4g Sabic polyphenylene ether resin SA90, and 350g organic solvent were added into a reactor, and stirred at 70°C and 350r / min for 40min until the mixture was dissolved and mixed uniformly to obtain a hot melt adhesive solution, wherein the organic solvent was a mixed solvent of ethanol and acetone, and the mass ratio of the solvent was 1:1;
[0038] S2. Preparation of moisture-curable hot-melt adhesive sheet
[0039] To the hot melt adhesive prepared in S1, 5 g of Covestro's polyisocyanate and 8 g of Evonik's Vestoplast 206 amorphous-α-polyolefin were added, and after being stirred and dispersed evenly, 60 μm was coated on a 100 μm double-sided release paper using a doctor blade coater or a CED coater. After complete drying, a release film was attached and rolled up. After complete aging, the release film was peeled off and rolled up from the back to obtain a moisture-curable hot melt adhesive sheet. Example 4
[0040] S1. Preparation of hot melt adhesive
[0041] 100g Guangzhou Suning 8620M polyamide resin, 20g Nan Ya epoxy resin 128 (bisphenol A epoxy resin), 10g Sabic polyphenylene ether resin SA90, and 500g organic solvent were added into a reactor, and stirred at 60°C and 300r / min for 50min until the mixture was dissolved and mixed uniformly to obtain a hot melt adhesive solution, wherein the organic solvent was a mixed solvent of ethyl acetate and butanone, and the mass ratio of the solvents was 1:1;
[0042] S2. Preparation of moisture-curable hot-melt adhesive sheet
[0043] Add 2 g of polycarbodiimide crosslinker XR-5580 and 18 g of Evonik Vestoplast 206 amorphous-α-polyolefin to the hot melt adhesive solution prepared in S1, stir and disperse evenly, and then use a knife coater or a CED coater to coat 100 μm on a 150 μm double-sided release paper. After complete drying, attach a release film and roll it up. After complete aging, peel off the release film and roll it up from the back to obtain a moisture-curable hot melt adhesive sheet. Example 5
[0044] S1. Preparation of hot melt adhesive
[0045] 100g of American Kraton 2291 polyamide resin, 17g of Nanya Synasia epoxy resin S-21 (aliphatic epoxy resin), 3g of Sabic polyphenylene ether resin SA90, and 430g of toluene were added into a reaction kettle, and stirred at 60°C and 300r / min for 60min until the mixture was dissolved and mixed uniformly to obtain a hot melt adhesive solution;
[0046] S2. Preparation of moisture-curable hot-melt adhesive sheet
[0047] 5 g of a crosslinking agent and 20 g of Vestoplast 206 amorphous-α-polyolefin were added to the hot melt adhesive prepared in S1, wherein the crosslinking agent was a mixture of isocyanate and glycidyl ether in a weight ratio of 1:1. After being stirred and dispersed evenly, 50 um was coated on a 75 um PET double-sided release film using a doctor blade coater or a CED coater. After drying completely, the release film was attached and rolled up. After ripening completely, the release film was peeled off and rolled up from the back to obtain a moisture-curable hot melt adhesive sheet. Comparative Example 1
[0048] The isocyanate curing agent N3390 produced by Covestro was not added, and the rest was exactly the same as in Example 1. Comparative Example 2
[0049] The other steps were exactly the same as those in Example 1 except that Vestoplast 206 amorphous α-polyolefin was not added.
[0050] The product performance of the moisture-curable hot-melt adhesive sheets in the above Examples 1-5 and Comparative Examples 1-2 was tested respectively. The specific test items and test methods are shown in Table 1 below, and the test results are shown in Table 2.
[0051] Table 1
[0052]
[0053] Table 2
[0054]
[0055] Among them, 120℃*120s*0.6Mpa hot pressing is used for the bonding strength test.
[0056] It can be seen from the experimental data in the above table that a moisture-curable hot-melt adhesive sheet material having excellent bonding strength to plastic plates and leather and a low drop in bonding strength after cold and hot shock and high-temperature boiling can be prepared by adding different ratios; the present invention uses a soluble polyamide resin with an epoxy resin and a low molecular weight polyphenylene ether resin containing a reactive group to react with a cross-linking agent to cross-link to form an interpenetrating network structure, thereby ensuring that the product has high bonding strength during initial hot pressing, and the addition of a moisture-curable polymer can further cross-link to achieve the purpose of post-stage curing, thereby improving the temperature resistance and hydrolysis resistance of the moisture-curable hot-melt adhesive sheet.
[0057] It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope limited by the appended claims of the application.
Claims
1. Moisture curable hot melt adhesive sheet, Features: It includes a release layer and a hot melt adhesive layer which are arranged in sequence; The hot melt adhesive layer is prepared by uniformly mixing polyamide resin, epoxy resin, hydrophobic active agent, organic solvent, crosslinking agent and moisture curing polymer in a weight ratio of 100: (5-20): (3-10): (300-600): (0.1-5): (5-25); The hydrophobic active agent is a polyphenylene ether resin containing a reactive group, and the weight average molecular weight of the polyphenylene ether resin is 1000-3000; The cross-linking agent is one or a mixture of two or more of polyisocyanate, polyamine and glycidyl ether; The moisture curing polymer is an amorphous-alpha-polyolefin containing siloxane.
2. The moisture-curable hot-melt adhesive sheet according to claim 1, Features: The thickness of the release layer is 25-150 μm, and the thickness of the hot melt adhesive layer is 25-100 μm.
3. The moisture-curable hot-melt adhesive sheet according to claim 1, Features: The epoxy resin is one of bisphenol A epoxy resin, bisphenol F epoxy resin or aliphatic epoxy resin.
4. The moisture-curable hot-melt adhesive sheet according to claim 1, Features: The epoxy value of the epoxy resin is 400-700 g / eq.
5. The moisture-curable hot-melt adhesive sheet according to claim 1, Features: The organic solvent is one or a mixed solution of two or more of ethanol, isopropanol, ethyl acetate, toluene, acetone and butanone.
6. The moisture-curable hot-melt adhesive sheet according to claim 1, Features: The polyamide resin is prepared by high-temperature condensation reaction of dimer acid and polyamine.
7. A method for producing a moisture-curable hot-melt adhesive sheet according to any one of claims 1 to 6, It is characterized in that The following steps are involved: S01. Preparation of hot melt adhesive The polyamide resin, epoxy resin, hydrophobic active agent and organic solvent are mixed in proportion, stirred at 50-70° C. and 250-350 r / min for 40-70 min, and the hot melt adhesive solution is obtained after the mixture is evenly mixed; S02. Preparation of moisture-curable hot-melt adhesive sheet A cross-linking agent and a moisture-curable polymer are added to the hot melt adhesive liquid prepared in step S01, stirred and dispersed evenly, and then filtered. After being coated on the release layer by a blade coater or a CED coater and dried completely, a release film is attached and rolled up for aging. After aging, the product is peeled off the release film on the composite and rolled up from the back to obtain a moisture-curable hot melt adhesive sheet.